1. Introduction

In the realm of precision investment casting, achieving high-quality cast components with minimal defects remains a critical challenge. Defects such as shrinkage porosity, microporosity, and deformation often arise due to complex interactions between process parameters, casting geometry, and material properties. This study focuses on optimizing the precision investment casting process for a stainless steel three-way valve body, which exhibited significant defects during production. By integrating numerical simulations with grey correlation analysis, we aim to identify the optimal combination of process parameters to enhance casting quality while reducing trial-and-error costs.

The term precision investment casting refers to a near-net-shape manufacturing technique renowned for producing intricate components with excellent surface finish. However, its sensitivity to process variables—such as pouring temperature, shell roasting temperature, and pouring time—demands systematic optimization. Traditional approaches rely heavily on empirical adjustments, which are time-consuming and resource-intensive. Here, we propose a data-driven framework that combines finite element simulations (via ProCAST) and statistical methods (grey correlation analysis) to streamline the optimization process.


2. Methodology

2.1 Problem Identification

The stainless steel three-way valve body, with a mass of 2.42 kg and varying wall thicknesses (4–24.96 mm), consistently exhibited defects in its original casting process. Shrinkage porosity (1.95 cm³) and deformation (0.0325 cm) were concentrated at thick-walled junctions, attributed to uneven heat dissipation and inadequate feeding during solidification (Figure 1).

2.2 Material and Simulation Setup

  • Material: SCS16 stainless steel (chemical composition in Table 1).
  • Simulation Software: ProCAST was used to model thermal behavior, utilizing thermophysical parameters for SCS16 and mullite ceramic shells (Figures 2a–2b).
  • Mesh Configuration: The original top-pouring system was discretized into 195,858 surface elements and 45,906 volume elements (Figure 3).

Table 1: Chemical Composition of SCS16 Stainless Steel (wt%)

CrSiMnPSNiMoFe
17–20<1.5<2<0.04<0.0412–162–3Bal.

2.3 Orthogonal Experimental Design

To systematically evaluate the effects of key parameters, an L9 orthogonal array was designed with three factors and three levels (Table 2). The quality objectives were shrinkage porosity volume and deformation amount.

Table 2: Factors and Levels for Orthogonal Experiments

LevelPouring Temperature (°C)Shell Roasting Temperature (°C)Pouring Time (s)
11,6101,0004
21,6401,0506
31,6701,1008

Table 3: Orthogonal Experiment Scheme (L9 Array)

TrialA (°C)B (°C)C (s)
11,6101,0004
21,6101,0506
31,6101,1008
41,6401,0006
51,6401,0508
61,6401,1004
71,6701,0008
81,6701,0504
91,6701,1006

3. Grey Correlation Analysis

3.1 Data Preprocessing

Raw experimental data were normalized using the following equation to eliminate dimensional differences:

where xixi​ is the original value and yiyi​ is the dimensionless value.

3.2 Grey Correlation Coefficient Calculation

The grey correlation coefficient (δiδi​) quantifies the similarity between experimental results and ideal outcomes:

where yi0yi0​ is the reference sequence, and ρ=0.5ρ=0.5 (distinguishing coefficient).

3.3 Entropy Weight Method

To objectively assign weights to quality objectives, entropy values (ejej​) and weights (wjwj​) were calculated:

Table 4: Weight Distribution for Quality Objectives

ObjectiveWeight (wjwj​)
Shrinkage Porosity0.2873
Deformation Amount0.7127

4. Results and Discussion

4.1 Grey Correlation Degree Ranking

The comprehensive grey correlation degree (GiGi​) for each trial was computed as:

Table 5: Grey Correlation Analysis Results

TrialShrinkage Porosity (cm³)Deformation (cm)GiGi​Rank
10.09540.03130.36607
20.05660.02390.92081
30.04460.03040.56443
40.07440.03200.38236
50.07140.03120.41155
60.09180.03130.36978
70.07110.02490.38494
80.10760.03220.33339
90.05610.02470.80882

The optimal parameters were identified as A1B2C2:

  • Pouring Temperature: 1,610°C
  • Shell Roasting Temperature: 1,050°C
  • Pouring Time: 6 s

4.2 Factor Significance Analysis

Grey correlation mean range analysis revealed the relative influence of factors:

Table 6: Mean Range Analysis of Process Parameters

ParameterMean Range (RR)Significance Rank
Pouring Time (C)0.34761
Pouring Temperature (A)0.22932
Shell Temperature (B)0.20333

This indicates that pouring time has the most significant impact on casting quality, followed by pouring temperature and shell temperature.


5. Validation and Industrial Application

Under the optimized parameters, the precision investment casting process demonstrated remarkable improvements:

  • Shrinkage Porosity: Reduced by 97% (from 1.95 cm³ to 0.0566 cm³).
  • Deformation: Reduced by 27% (from 0.0325 cm to 0.024 cm).

The modified gating system ensured sequential solidification, eliminating isolated liquid zones and enhancing feeding efficiency. Production trials confirmed defect-free castings with dimensional accuracy, validating the robustness of the grey correlation approach.


6. Conclusions

  1. Grey Correlation Analysis: A highly effective tool for optimizing precision investment casting parameters, requiring minimal experimental data while delivering reliable results.
  2. Optimal Parameters: Pouring temperature = 1,610°C, shell roasting temperature = 1,050°C, pouring time = 6 s.
  3. Factor Significance: Pouring system design exerts the greatest influence on quality, followed by pouring time and temperature parameters.

This study underscores the synergy between numerical simulations and statistical methods in advancing precision investment casting. Future work will explore multi-objective optimization algorithms to further refine process robustness.