A Multiaxial Stress Contact Fatigue Risk Prediction Model for Carburised and Quenched Straight Spur Gears

Gear contact fatigue failure, manifesting as micro-pitting, pitting, and spalling, is a critical bottleneck problem in high-power-density transmission systems. Our research focuses on developing a predictive model for carburised and quenched straight spur gears by deeply characterising the correlation between the strength gradient of the modified layer and the mechanical response of the meshing contact. We propose a coupled mathematical model that integrates the gradient bearing effect with a multi-axial fatigue criterion to predict the risk of contact fatigue.

1. Gear Meshing Contact Model

1.1 Equivalent Meshing Model

For a pair of straight spur gears with a contact ratio ε between 1 and 2, single and double tooth meshing occurs alternately along the line of action. At any meshing point, the curvature radii and contact semi-width can be derived using Bobillier’s theorem and Hertzian contact theory. The governing equations are:

$$
\begin{cases}
F = \frac{9549 P_0}{n R_{pm} \cos \alpha_{pm}} \\
b = \sqrt{\frac{4F}{\pi B} \frac{\rho_{pm} \rho_{qm}}{\rho_{pm} + \rho_{qm}} \left( \frac{1 – \nu_p^2}{E_p} + \frac{1 – \nu_q^2}{E_q} \right)} \\
\rho_{pm} = \frac{m z_p \cos \alpha \tan \alpha_{pm}}{2} \\
\rho_{qm} = \frac{m z_q \cos \alpha \tan \alpha_{qm}}{2}
\end{cases}
$$

Here, F is the load, P0 is the power, n is the rotational speed, b is the contact semi-width, B is the face width, ρpm and ρqm are the curvature radii of the driving and driven gears, ν and E represent Poisson’s ratio and Young’s modulus, m is the module, α is the pressure angle, and z is the number of teeth. This model allows for a direct calculation of the contact geometry for the straight spur gear pair.

1.2 Elastic Half-Plane Contact Model

The contact loads on the surface of a straight spur gear can be decomposed into normal and tangential components. Using a micro-element approach, the stress components at any internal point (x, z) are given by:

$$
\sigma_x = -\frac{2z}{\pi} \int_{x_1}^{x_2} \frac{p(t)(x-t)^2}{[(x-t)^2 + z^2]^2} dt – \frac{2}{\pi} \int_{x_1}^{x_2} \frac{q(t)(x-t)^3}{[(x-t)^2 + z^2]^2} dt
$$

$$
\sigma_z = -\frac{2z^3}{\pi} \int_{x_1}^{x_2} \frac{p(t)}{[(x-t)^2 + z^2]^2} dt – \frac{2z^2}{\pi} \int_{x_1}^{x_2} \frac{q(t)(x-t)}{[(x-t)^2 + z^2]^2} dt
$$

$$
\tau_{xz} = -\frac{2z^2}{\pi} \int_{x_1}^{x_2} \frac{p(t)(x-t)}{[(x-t)^2 + z^2]^2} dt – \frac{2z}{\pi} \int_{x_1}^{x_2} \frac{q(t)(x-t)^2}{[(x-t)^2 + z^2]^2} dt
$$

These singular integral equations are solved numerically by discretising the load into rectangular micro-elements.

1.3 Discrete Micro-Element Numerical Method

For a rectangular load element pj, the analytical solution for the x-direction stress is:

$$
\sigma_{xp} = -\frac{p_j}{\pi} \left[ \arctan\left(\frac{s – x}{z}\right) + \arctan\left(\frac{s + x}{z}\right) – \frac{z(s+x)}{r_1^2} + \frac{z(x-s)}{r_2^2} \right]
$$

A shape function Tp,j-i is defined to facilitate the superposition of loads from all n elements:

$$
T_{p,j-i} = -\frac{1}{\pi} \left[ \arctan\left(\frac{s – x_{ij}}{z_j}\right) + \arctan\left(\frac{s + x_{ij}}{z_j}\right) – \frac{z_j(s + x_{ij})}{r_1^2} + \frac{z_j(x_{ij} – s)}{r_2^2} \right]
$$

The total x-direction stress is then the sum of contributions from both normal and tangential loads:

$$
\sigma_{xi} = \sum_{j=1}^{n} \left( T_{p,j-i} p_j + T_{q,j-i} q_j \right)
$$

This method provides an accurate and computationally efficient solution for the stress field within the straight spur gear contact zone.

2. Performance Gradient and Fatigue Parameters

2.1 Hardness Gradient

Carburising and quenching create a hardened layer on the tooth surface of a straight spur gear, with a hardness gradient from the surface to the core. We use the Thomas empirical formula to model this gradient, which is parameterised by surface hardness, core hardness, and effective case depth (DCHD). The model is validated against measurements taken from a carburised straight spur gear, as shown in the following table for our test gear pair (m = 6.5 mm, zp/zq = 24/25).

Gear Pair Parameters for Model Validation
Parameter Symbol Value
Module m 6.5 mm
Number of Teeth (Pinion/Gear) zp/zq 24/25
Center Distance a 160 mm
Effective Face Width B 30 mm
Pressure Angle α 20°
Young’s Modulus E 210 GPa
Poisson’s Ratio ν 0.3

The hardness distribution HV(z) as a function of depth z is given by:

$$
HV(z) =
\begin{cases}
a_a z^2 + b_a z + c_a & 0 \leq z < \text{DCHD} \\
a_b z^2 + b_b z + c_b & \text{DCHD} \leq z < z_{core} \\
HV_{core} & z_{core} \leq z
\end{cases}
$$

2.2 Residual Stress Gradient

Residual compressive stresses induced by the heat treatment significantly influence the contact fatigue resistance of a straight spur gear. We model this residual stress profile σRS(z) using a statistical prediction model developed by the Gear Research Centre (FZG) at the Technical University of Munich:

$$
\sigma_{RS}(z) = \sigma_D + \frac{\sigma_z – \sigma_D}{1 + e^{-k(z + \delta)}}
$$

Where σD is the maximum compressive stress and σz is the maximum tensile stress. Our measurements on the gear tooth flank showed a good agreement with this model, with an average error of about 4.5% within the 0-1 mm depth range.

3. Dang Van Multiaxial Criterion for Load-Bearing Risk Prediction

We adopt the Dang Van multiaxial fatigue criterion to evaluate the risk of crack initiation in the straight spur gear. This criterion states that fatigue failure occurs when the shear stress amplitude Δτmax on a critical plane exceeds a linear function of the hydrostatic stress σH. The risk factor RFP (risk of failure parameter) is defined as:

$$
RFP(\alpha, t) = \frac{\Delta\tau_{\text{max}}(\alpha, t) + \kappa_D \sigma_H(t)}{\lambda}
$$

Here, κD and λ are material parameters determined from fully reversed bending and torsion fatigue limits. To account for the localised material properties of the carburised layer, we incorporate the residual stress gradient and the depth-dependent material strength (derived from the hardness gradient). The modified risk factor R’FP is:

$$
R’_{FP}(\alpha, z, t) = \frac{\Delta\tau_{\text{max}}(\alpha, z, t) + \kappa_D \left[ \sigma_H(z, t) + \sigma_{RS}(z) \right]}{\lambda(z)}
$$

Where λ(z) is the depth-dependent fatigue limit, directly correlated to the local hardness. A value of RFP < 1 indicates a safe condition, while RFP ≥ 1 predicts failure.

4. Results and Discussion

4.1 Internal Stress Fields

We performed a numerical analysis using our discrete element method for a straight spur gear under a contact stress of 1500 MPa and a coefficient of friction of 0.05. The analysis showed that the maximum shear stress occurs below the surface, which is a classic characteristic of Hertzian contact. The inclusion of a small tangential load shifted the location of the peak risk slightly away from the contact centre.

4.2 Material Thresholds from Dang Van Criterion

The Dang Van criterion was applied to predict the RFP distribution within the straight spur gear tooth. The maximum material utilisation rate was found not at the surface but at a sub-surface location. The following table summarises the effect of including the residual stress on the RFP value.

Effect of Residual Stress on Maximum RFP
Condition Max RFP Value Location (x, z) (mm)
Without Residual Stress 0.83 (-0.1, 0.4)
With Residual Stress 0.71 (-0.1, 0.4)

The inclusion of the compressive residual stress significantly reduced the RFP from 0.83 to 0.71, demonstrating its beneficial effect in mitigating fatigue risk. This confirms that the residual compressive stress enhances the shear resistance of the straight spur gear material.

5. Analysis of Characteristic Parameter Influence

5.1 Influence of Friction Coefficient

We investigated the effect of the friction coefficient (f) on the RFP distribution. The results are summarised in the following table.

Influence of Friction Coefficient on RFP
Friction Coefficient (f) Location of Max RFP Max RFP Value
0.0 Sub-surface, centre 0.75
0.1 Sub-surface, offset from centre 0.85
0.2 Near-surface, offset from centre 0.95

An increase in the friction coefficient caused the high-risk zone to migrate from the sub-surface towards the surface. This implies that under good lubrication (low friction), cracks are more likely to initiate in the sub-surface, leading to classical pitting. In contrast, poor lubrication (high friction) increases surface stresses, favouring surface-initiated cracks and micro-pitting. This finding aligns well with known failure mechanisms for straight spur gears.

5.2 Influence of Surface Hardness and Applied Load

We also analysed the influence of surface hardness (HVsurface) and the applied nominal pressure (P0). The results are presented below.

Influence of Surface Hardness and Load on Fatigue Risk
Parameter Value Effect on Max RFP Distribution
Surface Hardness (HV) 600 Baseline (0.80) Unchanged
670 Reduced (0.71) Unchanged
750 Further Reduced (0.65) Unchanged
Applied Load (MPa) 1500 Baseline (0.71) Sub-surface
1900 Increased (>1.0) Expanded to near-surface

Higher surface hardness effectively reduced the RFP value, thereby improving the gear’s load-carrying capacity without altering the location of the critical point. Applying a higher load significantly increased the risk, expanding the contact area and creating a region where the RFP exceeded 1.0, thereby accelerating contact fatigue failure. These results are consistent with experimental observations from gear fatigue tests.

6. Conclusions

We have successfully developed a multiaxial stress contact fatigue risk prediction model for carburised and quenched straight spur gears. The key findings are as follows:

  1. Our model, which integrates a performance gradient with the Dang Van multiaxial fatigue criterion, provides a rapid and accurate method for predicting the surface and sub-surface failure risk in straight spur gears.

  2. The hardness gradient in a carburised straight spur gear enhances its load-bearing capacity by strengthening the material’s fatigue parameters. The compressive residual stress gradient improves the shear resistance along the depth, mitigating the initiation of tear-type cracks. Both observations are consistent with the enhanced fatigue strength from surface hardening processes.

  3. The model’s analysis of characteristic parameters shows that an increased friction coefficient shifts the risk domain from the sub-surface to the surface. This predicts that good lubrication leads to sub-surface crack initiation (pitting), while poor lubrication promotes surface-initiated cracks (micro-pitting). An increase in the applied load expands the at-risk area, accelerating fatigue failure. These predicted influences are in complete agreement with the failure characteristics observed in actual gear testing.

  4. The proposed method offers an efficient analytical framework for assessing contact fatigue risk. For its application to other gear types, equivalent gear parameters can be used to perform the contact risk prediction.

Scroll to Top