Heat Transfer Simulation and Experimental Study of Straight Spur Gear in Atomized Gas Quenching

Atomized gas quenching is a novel heat treatment technology characterized by high heat transfer coefficient, good temperature uniformity, high critical heat flux density, and low circulation flow rate. Gears are critical components in mechanical equipment, requiring excellent wear resistance, high contact fatigue resistance, and bending fatigue performance. The quality of a gear directly affects the service life of the entire equipment, and it is largely determined by the gear material and its heat treatment process. Therefore, extensive research has been devoted to gear materials and heat treatment technologies worldwide. In this work, we focus on the heat transfer simulation and experimental investigation of a straight spur gear during atomized gas quenching.

Quenching is the most important step in heat treatment. During the quenching cooling process, temperature differences between the interior and exterior of the workpiece generate quenching stresses. To evaluate the microstructure transformation and residual stresses in the quenched workpiece, it is essential to determine the temperature evolution over time. Considering the influence of latent heat of phase transformation, we calculated the synthetical surface heat transfer coefficient of the straight spur gear during atomized gas quenching using MATLAB software. The transient temperature field of the straight spur gear during atomized gas quenching was numerically simulated using ANSYS finite element software. Corresponding experimental verification of the temperature field was also conducted.

1. Temperature Field Simulation of the Straight Spur Gear

1.1 Heat Conduction Equation in Quenching Process

Based on Fourier’s law of heat conduction and the principle of energy conservation, the heat conduction equation for the quenching process can be established. For a cylindrical coordinate system, the transient three-dimensional heat conduction differential equation with an internal heat source is expressed as:

$$
k \left( \frac{\partial^2 T}{\partial r^2} + \frac{1}{r} \frac{\partial T}{\partial r} + \frac{1}{r^2} \frac{\partial^2 T}{\partial \varphi^2} + \frac{\partial^2 T}{\partial z^2} \right) + q’ = c_p \rho \frac{\partial T}{\partial t} \tag{1}
$$

where \(k\) is the thermal conductivity, \(\rho\) is the material density (kg/m3), \(c_p\) is the specific heat at constant pressure (J/(kg·K)), \(r\) is the radius in cylindrical coordinates (m), \(\varphi\) is the azimuthal angle, and \(q’\) is the volumetric heat source density from internal heat generation (W/m3).

1.2 Boundary Conditions and Thermophysical Properties

In the atomized gas quenching process, the heat exchange between the workpiece and the cooling medium occurs on all surfaces. The boundary conditions for the end faces of the straight spur gear are given by:

$$
-\lambda \left. \frac{\partial T}{\partial r} \right|_{y=0} = h_1 (T_s – T_m) \tag{2}
$$

where \(\lambda\) is the thermal conductivity of the workpiece, \(h_1\) is the interface heat transfer coefficient at the medium side, \(T_s\) is the surface temperature of the workpiece, and \(T_m\) is the temperature of the cooling medium (atomized gas). The initial temperature of the workpiece is 860°C, and the cooling temperature of the atomized gas is 20°C.

For the lateral and top surfaces of the straight spur gear, the boundary conditions involve both radiation and natural convection. They are expressed as:

$$
-\lambda \left. \frac{\partial T}{\partial r} \right| = (h_2 + h_3)(T_s – T_a) \quad \text{and} \quad -\lambda \left. \frac{\partial T}{\partial y} \right|_{y=L} = (h_2 + h_3)(T_s – T_a) \tag{3}
$$

where \(T_a\) is the ambient temperature (20°C), \(h_2\) is the radiation heat transfer coefficient, and \(h_3\) is the natural convection heat transfer coefficient.

The material used for the straight spur gear is 45 steel. Its thermophysical properties, including specific heat and thermal conductivity at various temperatures, are listed in the following table.

Table 1: Thermophysical properties of 45 steel
Temperature \(T\) (°C) Specific heat \(c_p\) (J/(kg·K)) Thermal conductivity \(k\) (W/(m·K))
20 472 47.68
100 480 43.53
200 498 40.44
300 534 38.13
400 560 36.02
500 615 34.14
600 700 31.98
700 854 28.66
755 1064 25.14
800 806 26.49
900 637 25.92
1000 602 24.02

1.3 Treatment of Latent Heat of Phase Transformation

During atomized gas quenching, when the workpiece cools below the critical temperatures \(A_{c1}\) or \(A_{c3}\) of austenite, the Gibbs free energy of austenite becomes higher than that of the newly formed phases. This excess free energy provides the driving force for phase transformation. The austenite becomes unstable, and new phases with different compositions and morphologies appear. To account for the latent heat released during phase transformation, we employed the equivalent heat capacity method together with an equivalent internal heat source approach. This method is convenient, intuitive, and agrees well with actual quenching conditions.

Based on phase transformation kinetics, the TTT curve and the Scheil additivity rule are used to compute the volume fraction of each phase during cooling. The latent heat release rate is given by:

$$
q_\nu = \Delta H \frac{\Delta V’}{\Delta t} \tag{4}
$$

where \(\Delta t\) is the time step, \(\Delta V’\) is the incremental volume fraction of phase transformation during \(\Delta t\), and \(\Delta H\) is the enthalpy change of the corresponding phases (J/m3). The enthalpy change is calculated as:

$$
\Delta H = \int_{T_1}^{T_2} c_p \rho (T) \, dT \tag{5}
$$

The equivalent heat capacity method incorporates the latent heat into the apparent specific heat over the transformation temperature range.

1.4 Calculation of Synthetical Surface Heat Transfer Coefficient

The heat transfer during conventional quenching includes partial film boiling, nucleate boiling, natural convection, and radiation. The general heat transfer curve for metals and alloys during quenching is shown schematically in the literature. Based on the Leidenfrost transition model and the characteristics of atomized gas quenching, we wrote a finite difference program in MATLAB to compute the synthetical surface heat transfer coefficient for the straight spur gear under the given process parameters. The calculated variation of heat transfer coefficient with surface temperature is presented in the following table.

Table 2: Synthetical surface heat transfer coefficient vs. temperature for straight spur gear in atomized gas quenching
Temperature \(T\) (°C) Heat transfer coefficient \(h\) (W/(m2·K))
860 0.005
800 0.008
700 0.012
600 0.018
500 0.025
400 0.032
300 0.045
200 0.040
100 0.030
20 0.020

As shown, when the surface temperature of the straight spur gear cools from the initial 860°C to about 300°C, a large temperature difference exists between the workpiece and the medium. The medium near the surface is instantly heated and vaporized, forming a vapor film at the interface. This stage corresponds to film boiling, where the vapor film has poor thermal conductivity, hindering heat dissipation and resulting in a relatively low heat transfer coefficient. When the surface temperature drops from approximately 300°C to 20°C, the vapor film and bubbles collapse and disappear, leading to a sharp increase in the heat transfer coefficient.

1.5 Temperature Field Simulation Results and Analysis

We established a three-dimensional solid model of the straight spur gear (45 steel) and meshed it using ANSYS. The finite element model is shown in the following figure. (

) The transient temperature field during atomized gas quenching was simulated. Temperature distributions at different quenching times are described below.

At 10.3 seconds of atomized gas quenching, the maximum temperature is 860°C, located at the middle of the gear web, while the minimum temperature is 453.786°C at the tooth tip. During the initial cooling stage, the surface temperature of the tooth decreases rapidly, but the web remains hot. At 90.3 seconds, the maximum temperature is 855.238°C (still at the web), and the minimum temperature drops to 109.063°C at the tooth tip. The teeth cool much faster than the web. After 180 seconds, the minimum temperature reaches 44.753°C at the tooth tip, and the maximum temperature is 764.722°C. The tooth surface temperature is now close to the ambient gas temperature, while the web cools more slowly.

The heat flux vector diagram reveals that heat flows from the web toward the tooth ends. This pattern is consistent with the temperature distribution: the heat flux magnitude is larger in the web region, indicating that thermal energy is conducted from the central web to the teeth.

We tracked ten equidistant nodes from the tooth surface to the web center. The temperature evolution of these nodes over time is plotted. The results show that the tooth surface cools extremely rapidly, while the web temperature declines gradually. The temperature difference between the tooth tip and the web is significant at early stages but diminishes as quenching proceeds.

2. Experimental Study and Validation

2.1 Experimental Setup and Procedure

To validate the simulation, we conducted atomized gas quenching experiments on a straight spur gear made of 45 steel. A small hole was drilled on the workpiece surface, and a thermocouple was embedded to measure the temperature history. The gear was heated to 860°C in a furnace and held for sufficient time to achieve full austenitization. It was then transferred to the atomized gas quenching apparatus. The quenching medium was a mixture of nitrogen and water mist at 20°C. The experimental setup consisted of a gas supply system, a water injection system, a collection ring, and a workholder.

2.2 Comparison of Simulated and Measured Temperatures

We compared the computed temperature at a tooth surface node with the measured temperature from the thermocouple. The comparison is presented in the following table.

Table 3: Comparison of calculated and measured temperatures for straight spur gear tooth surface
Time (s) Calculated temperature (°C) Measured temperature (°C)
0 860 860
10 720 715
20 600 598
30 500 505
40 420 418
50 350 355
60 290 288
70 240 242
80 200 198
90 170 172
100 145 148
120 110 112
150 75 78
180 50 52

The calculated temperature curve agrees well with the experimental curve. Some minor fluctuations in the measured data are attributed to the release of latent heat during phase transformation and the inherent measurement noise. The overall good agreement confirms that the numerical approach used in this study is correct and feasible for simulating the temperature field of a straight spur gear during atomized gas quenching.

3. Conclusion

In this work, we successfully simulated the temperature field of a straight spur gear during atomized gas quenching using finite element analysis, with the heat transfer coefficient computed via an inverse method. The following conclusions can be drawn:

  • During atomized gas quenching, the tooth surface of the straight spur gear cools rapidly, while the web temperature drops more slowly. The maximum temperature always appears at the web, and the tooth tip cools fastest.
  • The synthetical surface heat transfer coefficient is low during the film boiling stage (high temperature range) and increases sharply after the vapor film collapses around 300°C.
  • The calculated temperature evolution matches well with experimental measurements, validating the numerical model. This method provides a reliable basis for predicting the thermal behavior of straight spur gears in atomized gas quenching and can be extended to other gear geometries and quenching media.

Future work will focus on incorporating phase transformation kinetics and stress analysis to simulate the final microstructure and residual stress distribution in the straight spur gear.

Scroll to Top