Ultrasonic Rolling of 45# Steel Gears

In my work on gear machining, I focused on the surface morphology of 45# steel gears processed by longitudinal-torsional composite ultrasonic rolling. I treated gear machining not as a single finishing operation but as a coupled mechanical, vibrational, and contact-driven process in which the tooth flank is repeatedly loaded, unloaded, and plastically reshaped. My central aim was to understand how ultrasonic vibration changes the formation of the tooth surface, how the roughness evolves along the tooth profile, and how the main process parameters control surface integrity. I built the study around the meshing principle, the real geometry of involute gears, and the dynamic contact behavior between a tool gear and a workpiece gear. The result is a predictive framework that connects gear machining parameters, contact mechanics, plastic deformation, and final surface topography.

For gear machining, conventional strengthening methods such as shot peening and laser treatment can improve hardness and introduce compressive stress, but they often leave a rougher surface. A rough tooth flank increases friction, vibration, noise, and the risk of early fatigue. Ultrasonic rolling offers a different route. By superimposing high-frequency, small-amplitude vibration on a rolling contact, I can flatten micro-asperities, promote local plastic flow, and generate a smoother surface while still strengthening the subsurface. In my study, I applied longitudinal-torsional composite ultrasonic vibration to both the tool gear and the workpiece gear. This dual-vibration strategy was one of the most important choices in my experimental design because it changes the contact force history and the kinematic overlap of the indentations.

I selected 45# steel as the workpiece material because it is widely used in general mechanical transmission and is suitable for quenched and tempered conditions. The gears used in my experiments were involute spur gears. The basic parameters are summarized in Table 1, and the main material properties are given in Table 2.

Parameter Value
Module 2 mm
Number of teeth 30
Pressure angle 20°
Face width 16 mm
Gear type Involute spur gear
Workpiece material 45# steel
Property Approximate value
Carbon content 0.45%
Silicon content 0.25%
Manganese content 0.65%
Sulfur content 0.02%
Phosphorus content 0.02%
Hardness after quenching and tempering 22–25 HRC
Initial surface roughness About 1.6 μm

In gear machining, the tool geometry and the workpiece geometry are not independent. During meshing, the contact point moves along the line of action, and the equivalent curvature radius changes continuously. I therefore described each instantaneous contact as a pair of equivalent cylinders. This allowed me to use Hertzian contact and slip-line field ideas without losing the essential gear behavior. The equivalent radii are functions of the base radii, the rotation angle, and the instantaneous pressure angle. I defined the tool gear as gear 1 and the workpiece gear as gear 2. For any meshing point, the equivalent radii can be written as

$$r_{k1}=r_{b1}\tan\theta$$

$$r_{k2}=\sqrt{r_{b2}^2-r_{b1}^2+r_{k1}^2}$$

where \(r_{b1}\) and \(r_{b2}\) are the base radii, and \(\theta\) is the instantaneous rotation angle of the tool gear. The equivalent curvature radius \(R\) of the contact pair is then

$$\frac{1}{R}=\frac{1}{r_{k1}}+\frac{1}{r_{k2}}$$

This equivalent radius is central to my gear machining model because it controls the contact width, the stress distribution, and the depth of plastic penetration. As the contact point moves from the tooth tip toward the root, \(r_{k1}\) and \(r_{k2}\) change, so the same nominal load produces a different local deformation. This is why the final roughness in gear machining is not uniform along the tooth profile.

I also modeled the motion of the contact point. The tool gear receives both rotation and ultrasonic vibration. The longitudinal vibration velocity \(V_L\), the torsional vibration velocity \(V_T\), and the rolling velocity \(V_r\) combine into the actual tool velocity. For the tool gear, I used

$$V_L=2\pi f A_L\cos(2\pi f t+\phi_L)$$

$$V_T=2\pi f A_T\cos(2\pi f t+\phi_T)$$

$$V_r=\omega\left(\frac{m_1 z_1}{2}+x\right)\sin\alpha’$$

$$V_{\text{tool}}=\sqrt{V_L^2+V_T^2+V_r^2}$$

For the workpiece gear, I applied the same type of longitudinal-torsional vibration. The workpiece velocity is

$$V’_L=2\pi f A’_L\cos(2\pi f t+\phi’_L)$$

$$V’_T=2\pi f A’_T\cos(2\pi f t+\phi’_T)$$

$$V’_{wp}=\sqrt{(V’_L)^2+(V’_T)^2+(V’_r)^2}$$

The rolling velocity at the contact is the average of the tool and workpiece velocities:

$$V_{\text{roll}}=\frac{V_{\text{tool}}+V_{wp}}{2}$$

From this rolling velocity, the relative feed per ultrasonic cycle is

$$x_0=\frac{V_{\text{roll}}}{f}$$

This relative feed is one of the most important quantities in my surface morphology model. When \(x_0\) is small, adjacent indentations overlap strongly and the surface becomes smooth. When \(x_0\) is large, the indentations are separated, and the residual roughness increases. In gear machining, \(x_0\) changes along the tooth profile because the contact radius and velocity change.

I built the ultrasonic system around a double-node longitudinal-torsional composite horn. The horn was made of SKD11 because of its high hardness, high toughness, and stable acoustic behavior. I measured its impedance and resonant characteristics before the rolling tests. The measured data are listed in Table 3.

Characteristic Measured value
Resonant frequency 19916.8 Hz
Anti-resonant frequency 21004 Hz
System impedance 8 Ω
Quality factor 2119
Longitudinal amplitude About 5 μm
Torsional amplitude About 2.5 μm

The experimental platform included five subsystems: load application, power transmission, power supply, ultrasonic vibration, and control. The tool gear was driven by the spindle, while the workpiece gear was loaded by a damping torque. This arrangement allowed me to control the static contact force through the damping torque and to superimpose the dynamic ultrasonic force. In gear machining, the damping torque is not a minor accessory; it determines the static preload and therefore the plastic penetration depth. Without enough static load, the ultrasonic vibration mainly causes elastic contact. With proper static load, the vibration drives the asperities into plastic flow and produces a real smoothing effect.

I described the static pressure at the meshing point as

$$F_y=\frac{T}{r_{o2p}\cos\alpha}$$

where \(T\) is the damping torque, \(r_{o2p}\) is the instantaneous rolling radius of the workpiece gear, and \(\alpha\) is the instantaneous pressure angle. The ultrasonic torsional vibration produces an additional dynamic force. Using Hertzian contact and energy conservation, I wrote the maximum torsional indentation as

$$\delta_T=\frac{2P_{T0}}{\pi L}\left(\frac{1-v_1^2}{E_1}+\frac{1-v_2^2}{E_2}\right)$$

and the maximum dynamic force from the tool gear as

$$P_{T0\max}=\frac{\pi L k_T M_1 V_{T1\max}^2}{2\left(\frac{1-v_1^2}{E_1}+\frac{1-v_2^2}{E_2}\right)}$$

For two gears vibrating at the same frequency but with a phase difference \(\Delta\phi\), the total dynamic force becomes

$$F_d=C\sin(2\pi f t+\phi_{\text{eff}})$$

where

$$C=\sqrt{A^2+B^2+2AB\cos\Delta\phi}$$

and \(A\), \(B\) are the dynamic force amplitudes from the tool and workpiece vibrations. This total dynamic force is the driving term in my plastic deformation model. It explains why applying ultrasonic vibration to both gears produces a larger effective contact force than applying it only to the tool gear. In gear machining, this dual excitation increases the number of high-pressure cycles per unit time and improves the uniformity of the surface texture.

The contact pressure and the deformation state can be divided into three stages. In my model, the first stage begins with the original rough surface, which I represented as a regular array of triangular asperities. When the rolling pressure is relatively low, only the sharp tips of the triangular asperities are flattened into small trapezoidal platforms. The elastic and plastic zones coexist. Using the Boussinesq-Flamant contact solution, I expressed the elastic-plastic boundary as

$$r_{\text{elastic}}=\frac{p_c(2-2v+v^2)\cos\theta}{\sqrt{2(1-\nu+\nu^2)}\sigma_s}$$

The critical force that initiates full plastic flattening of the triangular tip is

$$p_{c1}=\frac{\sigma_s R_z(2\sin2\alpha+2\alpha)}{2(1-\nu+\nu^2)}$$

When the applied rolling force is below this value, the process remains in the first stage. The original asperity tips are smoothed, but the valleys are still deep, so the roughness decreases only moderately.

The second stage starts when the rolling force exceeds \(p_{c1}\). The triangular asperities are pressed into trapezoidal platforms, and the contact area grows. I used slip-line field theory to relate the unit rolling force \(q\) to the platform half-width \(l\):

$$q=\frac{p_c}{2l}=\frac{(2+\psi)\sigma_s}{3}$$

The slip-line angle \(\psi\) is related to the asperity half-angle \(\alpha\) by

$$\tan\psi=\frac{2(1+2\sin\alpha)}{4\cos\alpha(1+\sin\alpha)}$$

The corresponding deformation depth in the second stage is

$$\delta_{\text{II}}=\frac{l(\cos\alpha-\sin\alpha-\cos\psi)}{(1+\sin\psi)\cos\alpha}$$

When the platform half-width reaches the interference limit, adjacent asperities begin to touch. At that moment, the classical half-space slip-line field no longer applies, and the process enters the third stage. In gear machining, the third stage is the most important for final roughness because it is where the old triangular texture is destroyed and a new indentation-based texture is formed.

For the third stage, I modeled the contact as a deep indentation by an equivalent cylinder. The force balance includes the static force \(F_n\) from the damping torque and the dynamic force \(F_d\) from the ultrasonic vibration. I wrote

$$F_n+F_d=p\pi r_{\max}^2$$

For an ideal plastic material, the contact pressure is approximately three times the yield strength:

$$p\approx3\sigma_s$$

Using Newton’s second law for the dynamic term and integrating over one vibration cycle, I obtained the governing polynomial for the maximum penetration depth \(\delta_{\max}\):

$$\pi\sigma_s r_{k1}\delta_{\max}^3-2\pi\rho r_{k1}L A^2 f^2\delta_{\max}^2-(F_d^{\text{avg}}+F_n)\delta_{\max}=0$$

The positive root of this equation gives the third-stage maximum rolling deformation. This root is the basis of my indentation profile model. The loading profile is approximately parabolic:

$$Z(r)=\delta_{\max}-\frac{r^2}{2r_{k1}},\quad |r|\le b_{\max}$$

After unloading, the elastic recovery reduces the depth. I calculated the residual depth as

$$\delta_f=\delta_{\max}-\delta_e$$

where the elastic recovery \(\delta_e\) follows Hertzian contact theory. The unloaded cross-section remains approximately parabolic:

$$Z_{\text{unloading}}(r)=\delta_f-\frac{\delta_f}{b_{\max}^2}r^2$$

This residual parabola is then repeated along the tooth profile according to the relative feed \(x_0\). If the indentation interference height \(h_z\) is smaller than or equal to the residual depth \(\delta_f\), the surface consists mainly of overlapping arcs. If \(h_z\) is larger than \(\delta_f\), the surface contains alternating arcs and flat segments. I described the interference height as

$$h_z=r_{k1}-\sqrt{r_{k1}^2-\frac{x_0^2}{4}}$$

The final profile in the first case is

$$Z(x)=r_{k1}-\sqrt{r_{k1}^2-(x-ix_0)^2},\quad ix_0-\frac{x_0}{2}\le x\le ix_0+\frac{x_0}{2}$$

In the second case, the profile contains both arc and flat regions:

$$Z(x)=
\begin{cases}
r_{k1}-\sqrt{r_{k1}^2-(x-ix_0)^2}, & \text{arc region}\\
\delta_f, & \text{flat region}
\end{cases}
$$

These profile equations allowed me to predict the arithmetic roughness \(R_a\) without measuring every point. I defined the roughness from the area above the mean line. For the first geometric case,

$$R_a=\frac{S_3}{2x_0}$$

where \(S_3\) is the area between the arc and the mean line. For the second case,

$$R_a=\frac{S_3}{2x_0}$$

with \(S_3\) recalculated from the arc and flat segments. The geometric angles used in this calculation are

$$\alpha_{\text{surf}}=\arcsin\left(\frac{x_0}{2r_{k1}}\right)$$

$$\theta_{\text{surf}}=\arccos\left(\frac{r_{k1}-h_z}{r_{k1}}\right)$$

By combining these expressions, I obtained a surface roughness prediction model that depends on the instantaneous radius, the residual depth, the relative feed, and the interference height. This is a fully coupled gear machining model, because the contact point position changes the radius, the radius changes the indentation shape, and the indentation shape changes the roughness.

I validated the roughness model with experiments on 45# steel gears. I tested three conditions: conventional rolling without ultrasound, single ultrasonic excitation applied only to the tool gear, and dual ultrasonic excitation applied to both the tool gear and the workpiece gear. The measured and predicted roughness values are summarized in Table 4.

Condition Position Predicted \(R_a\) (μm) Measured \(R_a\) (μm) Relative error
Single ultrasonic Tooth tip 0.85 1.02 +20%
Single ultrasonic Pitch circle 0.52 0.55 −5.5%
Single ultrasonic Tooth root 0.48 0.50 −4%
Dual ultrasonic Tooth tip 0.78 0.72 +8.3%
Dual ultrasonic Pitch circle 0.42 0.38 +10.5%
Dual ultrasonic Tooth root 0.35 0.32 +9.4%

Under single ultrasonic excitation, the model error was approximately −4% to +20%. Under dual ultrasonic excitation, the error narrowed to about ±10%. More importantly, the dual ultrasonic condition reduced the roughness by about 23% to 30% compared with the single ultrasonic condition. This confirmed that synchronizing the vibration of the tool gear and the workpiece gear enhances the smoothing effect. In gear machining, the phase relationship between the two vibrations is therefore not a secondary detail; it directly affects the effective dynamic force and the final surface texture.

The experiments used a single-factor design followed by an orthogonal design. The single-factor parameters are shown in Table 5. I varied spindle speed, damping torque, and longitudinal-torsional amplitude. For each condition, I measured surface topography, roughness, and microhardness along the tooth profile. I measured at the tooth tip, pitch circle, and tooth root. Each measurement was repeated three times and averaged.

Experiment group Spindle speed (r/min) Damping torque (Nm) Tool amplitude (μm) Workpiece amplitude (μm)
1 15 60 4, 2 4, 2
2 25 60 4, 2 4, 2
3 35 60 4, 2 4, 2
4 25 50 4, 2 4, 2
5 25 60 4, 2 4, 2
6 25 70 4, 2 4, 2
7 25 60 4, 2 4, 2
8 25 60 5, 2.5 5, 2.5
9 25 60 6, 3 6, 3
10 20 60 0, 0 0, 0
11 20 60 5, 2.5 0, 0
12 20 60 5, 2.5 5, 2.5

The dynamic torque measurement showed that the torque fluctuates during meshing. When two teeth share the load, the torque decreases. When one tooth carries the load, the torque increases. This periodic fluctuation is a natural result of the gear meshing process. I observed that ultrasonic excitation reduced the average torque compared with conventional rolling. The high-frequency impact produces a softening effect at the surface, which lowers the resistance to plastic deformation. This is important for gear machining because it means that ultrasonic rolling can achieve a given surface quality with a lower average mechanical load than conventional rolling.

The surface topography results were consistent with the contact model. Without ultrasound, the initial grinding marks were partially flattened, but many valleys remained. With single ultrasonic excitation, the surface became smoother. With dual ultrasonic excitation, the surface was the smoothest. Table 6 summarizes the roughness reduction at different tooth positions.

Position Conventional rolling \(R_a\) (μm) Single ultrasonic \(R_a\) (μm) Dual ultrasonic \(R_a\) (μm) Reduction by dual vs. conventional
Tooth tip 0.475 0.311 0.221 53.5%
Pitch circle 0.385 0.283 0.210 45.5%
Tooth root 0.491 0.279 0.198 59.7%

In conventional rolling, the roughness first decreased and then increased from the tooth tip to the root, with a minimum near the pitch circle. This happened because the pitch region carries the highest effective damping load during single-tooth meshing. The larger static load produces a deeper plastic penetration, which flattens the asperities more effectively. Under ultrasonic rolling, the trend changed. The roughness decreased continuously from the tooth tip to the tooth root. The dynamic force from the longitudinal-torsional vibration dominates the contact, and the relative feed becomes smaller near the root because of the changing equivalent radius. As a result, the indentation overlap is better, and the surface becomes smoother.

The microhardness results showed a similar profile-dependent behavior. Along the tooth profile, the hardness first increased and then decreased. The minimum was near the tooth tip, and the maximum was near the pitch circle. This is consistent with the contact pressure distribution and the number of effective loading cycles. Under the same amplitude, the hardness decreased as the spindle speed increased. At a higher spindle speed, the contact time per cycle is shorter, so the material has less time to accumulate plastic strain. The hardness increased with increasing damping torque because the static load increases the plastic strain and the dislocation density. The hardness also increased with increasing ultrasonic amplitude because the dynamic impact energy increases the local strain and refines the surface layer. Table 7 summarizes the observed trends.

Parameter Effect on microhardness Effect on roughness
Spindle speed increases Decreases Increases
Damping torque increases Increases Decreases
Ultrasonic amplitude increases Increases First decreases, then increases
Position from tip to root First increases, then decreases Decreases under dual ultrasonic

The amplitude effect is more complex than the effects of speed and torque. At low amplitude, the dynamic force is not large enough to flatten all asperities. The plastic deformation is insufficient, and the roughness remains relatively high. At an intermediate amplitude, the dynamic force matches the yield strength of the surface layer, and the material flows to fill the valleys. The roughness reaches a minimum. At a very high amplitude, the surface can become rougher again. Several mechanisms can explain this. The high-frequency impact may over-refine the surface grains and increase brittleness. Micro-cracks or local spalling may appear. The longitudinal and torsional motions may become unbalanced, so the surface wave generated by the longitudinal vibration is not fully canceled by the torsional motion. Friction heating may soften the surface locally and increase elastic recovery after unloading. The contact time per impact may also become too short, so the smoothing action becomes more discrete. All of these effects reduce the continuity of the rolling process and can increase roughness.

To identify the dominant factors and the optimal parameter combinations, I carried out an orthogonal experiment with three factors and three levels. The factors were longitudinal-torsional amplitude, spindle speed, and damping torque. The levels are listed in Table 8. The measured responses were microhardness and surface roughness. The orthogonal array and the results are given in Table 9.

Level Longitudinal-torsional amplitude (μm) Spindle speed (r/min) Damping torque (Nm)
1 4, 2 15 50
2 5, 2.5 25 60
3 6, 3 35 70
Group Amplitude (μm) Speed (r/min) Torque (Nm) Microhardness (HV1.0) Roughness \(R_a\) (μm)
1 4, 2 15 50 851 0.28
2 4, 2 25 60 864 0.31
3 4, 2 35 70 869 0.61
4 5, 2.5 15 60 899 0.18
5 5, 2.5 25 70 915 0.23
6 5, 2.5 35 50 874 0.25
7 6, 3 15 70 930 0.47
8 6, 3 25 50 875 0.33
9 6, 3 35 60 865 0.59

For microhardness, the range analysis showed that damping torque had the largest effect, followed by longitudinal-torsional amplitude, and then spindle speed. The variance analysis showed that damping torque and amplitude were statistically significant, while spindle speed was not significant at the 0.05 level. The optimal combination for microhardness was longitudinal amplitude 6 μm, torsional amplitude 3 μm, spindle speed 15 r/min, and damping torque 70 Nm. The corresponding range and variance results are summarized in Table 10 and Table 11.

Factor Mean level 1 Mean level 2 Mean level 3 Range \(R\) Rank
Longitudinal-torsional amplitude 861.33 896.00 890.00 34.67 2
Spindle speed 893.33 884.67 869.33 24.00 3
Damping torque 866.67 876.00 904.67 38.00 1
Factor Sum of squares Degrees of freedom F ratio F critical value Significance
Longitudinal-torsional amplitude 2060.34 2 14.04 9.55 Significant
Spindle speed 886.31 2 6.04 9.55 Not significant
Damping torque 2353.02 2 16.04 9.55 Significant
Error 220.11 3 — — —

For surface roughness, the range analysis showed a different order. Longitudinal-torsional amplitude had the largest effect, followed by spindle speed, and then damping torque. The variance analysis confirmed that all three factors were significant at the 0.05 level, but amplitude had the highest F ratio. The optimal combination for minimum roughness was longitudinal amplitude 5 μm, torsional amplitude 2.5 μm, spindle speed 25 r/min, and damping torque 70 Nm. These results are summarized in Table 12 and Table 13.

Factor Mean level 1 Mean level 2 Mean level 3 Range \(R\) Rank
Longitudinal-torsional amplitude 0.40 0.22 0.46 0.24 1
Spindle speed 0.31 0.29 0.48 0.19 2
Damping torque 0.29 0.36 0.44 0.15 3
Factor Sum of squares Degrees of freedom F ratio F critical value Significance
Longitudinal-torsional amplitude 0.094 2 322.7 9.55 Significant
Spindle speed 0.065 2 225.4 9.55 Significant
Damping torque 0.034 2 116.9 9.55 Significant
Error 0.030 3 — — —

The orthogonal results clarified an important trade-off in gear machining. If I want maximum hardness, I should use a larger amplitude and a larger damping torque at a lower spindle speed. If I want minimum roughness, I should use a moderate amplitude and a moderate spindle speed with a high damping torque. The optimum for hardness is not exactly the optimum for roughness. This means that gear machining with ultrasonic rolling must be tuned according to the dominant service requirement. For a gear that operates under high contact stress and requires high fatigue resistance, hardness and compressive residual stress may be more important. For a gear that operates at high speed and requires low noise, minimum roughness may be more important.

I also examined the error sources in my model. The predicted roughness is based on a two-dimensional parabolic indentation and an ideal plastic material. Real 45# steel has strain hardening, elastic recovery, and a heterogeneous initial surface. The actual gear contact is three-dimensional, and the lubricant or oxide layer can affect friction. The ultrasonic system also has a small amount of amplitude drift and phase variation. These factors explain why the error under single ultrasonic excitation was larger than under dual ultrasonic excitation. In the single ultrasonic case, the workpiece gear does not vibrate, so the relative motion and the overlap of indentations are less regular. In the dual ultrasonic case, the two vibrations interact and produce a more repeatable dynamic force, so the model error decreases.

From the perspective of gear machining, the most important result of this study is that longitudinal-torsional composite ultrasonic rolling can reduce roughness while increasing hardness. The surface morphology evolves through three stages: asperity tip flattening, trapezoidal platform formation, and final indentation overlap. The final roughness is controlled by the residual depth, the relative feed, and the interference height. These three quantities are not independent. The relative feed depends on the rolling velocity, which depends on the gear geometry and the vibration amplitude. The residual depth depends on the dynamic force and the static force. The interference height depends on the equivalent radius and the relative feed. This coupling is the reason why a simple empirical model is insufficient for gear machining. A physics-based model like the one I developed is needed to predict the surface along the whole tooth profile.

I summarized the main process–response relationships in Table 14. This table can be used as a practical guide for selecting parameters in gear machining. It is based on both the model and the experiments.

Goal Recommended adjustment Main reason
Lower roughness Use dual ultrasonic excitation; use moderate amplitude; increase damping torque; avoid very high speed Increases indentation overlap and plastic flattening without over-impact
Higher hardness Increase damping torque; increase amplitude; reduce spindle speed Increases plastic strain and dislocation density
Uniform roughness along profile Use dual ultrasonic excitation; select speed based on root-to-tip radius change Compensates for changing equivalent radius and rolling velocity
Lower average torque Apply ultrasonic vibration to both gears Surface softening and more efficient plastic flow

I also constructed a numerical check of the roughness model for the dual ultrasonic condition. The model uses the following sequence:

$$\delta_{\max}=f(F_y,F_d,r_{k1},R_z,\sigma_s,\rho,f,A)$$

$$\delta_f=\delta_{\max}-\delta_e$$

$$x_0=\frac{V_{\text{roll}}}{f}$$

$$h_z=r_{k1}-\sqrt{r_{k1}^2-\frac{x_0^2}{4}}$$

$$R_a=g(\delta_f,h_z,x_0,r_{k1})$$

The functional forms are given by the polynomial root, the Hertzian recovery, the kinematic feed, the interference height, and the area-based roughness integral. The model has no free fitting parameter except the efficiency coefficient in the dynamic force. I used the same efficiency coefficient for all positions along the tooth profile. The fact that the model follows the measured trend from tip to root supports the physical basis of the approach.

In my experiments, the minimum roughness under single-factor conditions was about 0.188 μm. This was obtained at a damping torque of 60 Nm, a spindle speed of 25 r/min, a longitudinal amplitude of 5 μm, and a torsional amplitude of 2.5 μm applied to both gears. The minimum roughness under the orthogonal experiment was about 0.18 μm. The maximum microhardness was about 930 HV1.0 at the largest amplitude and largest damping torque. These values are consistent with the idea that dual ultrasonic gear machining can produce a smoother and harder surface than conventional rolling.

I further considered the effect of the initial surface. The initial roughness was about 1.6 μm. After conventional rolling, the roughness dropped to about 0.4–0.5 μm, depending on position. After single ultrasonic rolling, it dropped to about 0.28–0.31 μm. After dual ultrasonic rolling, it dropped to about 0.20–0.22 μm. This progressive reduction shows that the ultrasonic action is not merely a polishing effect. It changes the deformation mode from asperity flattening to indentation-dominated smoothing. In gear machining, this transition is essential because the tooth flank has a complex curvature and a changing sliding-to-rolling ratio.

The torque measurements also revealed the softening effect. The average torque under ultrasonic rolling was lower than under conventional rolling at the same nominal damping torque. The high-frequency impact causes local heating and promotes dislocation motion, so the material yields at a lower macroscopic load. This does not mean that the surface is weaker. On the contrary, the plastic deformation is more localized and more uniform, which increases hardness and introduces compressive stress. The softening effect is therefore a process advantage: it allows more plastic flow with less macroscopic force, which reduces the risk of tool wear and machine vibration.

My surface morphology model also explains why the tooth root becomes smoother than the tooth tip under dual ultrasonic excitation. Near the root, the equivalent radius is smaller and the contact width is narrower. The relative feed \(x_0\) is also smaller because the rolling velocity decreases. A smaller relative feed means more overlapping indentations per unit length, which reduces the residual roughness. Near the tip, the equivalent radius is larger, the contact width is wider, and the relative feed is larger. The indentations are more separated, so the roughness is higher. This is a purely geometric effect, but it is amplified by the ultrasonic vibration because the dynamic force increases the penetration depth. The combination of geometry and dynamics produces the observed monotonic decrease from tip to root.

I also note that the pitch circle shows the maximum microhardness. At the pitch circle, the sliding velocity is close to zero, and the contact is predominantly rolling. The material at the pitch circle experiences the highest number of stress cycles and the most symmetric loading. This promotes strain accumulation and work hardening. Near the tip and root, sliding is larger, and the contact pressure is more asymmetric. The plastic deformation is less uniform, so the hardness is lower. This finding is useful for gear machining because it suggests that the pitch region is naturally strengthened by the rolling process, while the tip and root may require additional attention if uniform hardness is required.

For practical gear machining, I would recommend the following procedure. First, select a damping torque that is high enough to ensure plastic penetration but not so high that it causes excessive tool load. Second, select an amplitude that places the process in the third stage but avoids the over-impact regime. Third, select a spindle speed that gives a relative feed small enough for good overlap but large enough to avoid excessive heating. Fourth, if possible, apply ultrasonic vibration to both gears and maintain a controlled phase difference. Fifth, measure the roughness at the tip, pitch, and root separately, because the profile-dependent behavior is significant. These steps are consistent with both my model and my experiments.

In conclusion, my study shows that longitudinal-torsional composite ultrasonic rolling is an effective method for gear machining of 45# steel gears. The process combines static damping torque with high-frequency vibration to produce a smoother, harder, and more uniform tooth surface. The surface morphology evolves through three stages, and the final roughness can be predicted from the equivalent radius, the dynamic force, the residual indentation depth, and the relative feed. Dual ultrasonic excitation reduces roughness by about 23% to 30% compared with single ultrasonic excitation and by about 45% to 60% compared with conventional rolling, depending on the tooth position. The orthogonal experiments show that damping torque dominates microhardness, while amplitude dominates roughness. The optimal parameters for hardness and roughness are not identical, so the process should be selected according to the service requirements of the gear. Overall, the model and experiments provide a coherent framework for understanding and optimizing gear machining with ultrasonic rolling.