Gear Cold Extrusion Die Failure Analysis and Design Method

I have focused my research on the cold extrusion of a straight-tooth cylindrical gear used in a heavy-duty vehicle wheel-side reducer. The central problem is that cold extrusion can produce a high-quality forged gear blank with continuous metal flow lines, high material utilization, short processing chains, and good mechanical properties, but the die itself is subjected to extremely high forming loads. These loads can cause cracking, fracture, wear, and other failure modes. My work therefore combines theoretical design, finite element simulation, response surface optimization, and process experiments to develop a die structure that can prevent early failure and support industrial production of a forged gear blank.

1. Introduction

Gears are among the most common transmission components in mechanical systems. In automotive and motorcycle applications, they must transmit power, change speed, and alter torque direction under complex working conditions. Traditional cutting processes are mature and stable, but they require long processing times, remove a large amount of material, interrupt the metal flow lines, and increase production cost. For high-volume manufacturing, these disadvantages become significant. Cold extrusion, by contrast, forms a forged gear blank at room temperature by forcing metal to flow plastically into a die cavity. The process offers high efficiency, low energy consumption, high material utilization, and improved strength because the metal flow lines remain continuous.

However, cold extrusion of gears also creates severe loading on the die. The concave die, or die insert, is the main load-bearing component. It experiences high internal pressure, friction, cyclic loading, and stress concentration. When the tensile stress in the die insert exceeds the material limit, cracks or fractures can appear. This failure limits the wider application of cold extrusion to gear manufacturing. My research therefore aims to understand the failure mechanisms of gear cold extrusion dies and to propose a reliable design method that avoids early failure and extends die life.

The specific object of my study is a straight-tooth cylindrical planetary gear. It has an external tooth profile and a central hole. The gear is made of 20CrMnTi, which has good plasticity and is suitable for cold extrusion. I use a forward extrusion scheme to form the external teeth and the inner hole in one operation. The resulting forged gear blank can reduce material waste, shorten the process chain, and lower production cost. The key challenge is that the forming load is very large, and the die insert must be designed to withstand that load without failure.

2. Research Object and Forming Scheme

I first analyzed the geometric characteristics of the gear. The gear is a straight-tooth cylindrical gear with a module of 4.1 mm, 18 teeth, a pressure angle of 22.5 degrees, and a modification coefficient of 0.366. The tip circle diameter is 83.09 mm, the root circle diameter is 67.37 mm, and the inner hole diameter is 44.95 mm. These parameters define the die cavity and the billet dimensions. The material is 20CrMnTi, and its flow stress curve is used in the finite element simulation.

Parameter Value
Module, m 4.1 mm
Number of teeth, z 18
Pressure angle, α 22.5°
Modification coefficient, x 0.366
Tip circle diameter 83.09 mm
Root circle diameter 67.37 mm
Inner hole diameter 44.95 mm
Material 20CrMnTi

I selected a forward extrusion process. In this scheme, the billet is placed in the die cavity. The upper punch moves downward, while the lower punch remains fixed. The external teeth are formed as the metal flows through the die opening, and the inner hole is formed by the lower punch. After extrusion, the upper punch retracts, and the forged gear blank is ejected by the ejector. This process can form the external teeth and the inner hole in one stroke, which reduces the number of operations and improves production efficiency.

The die materials must have high hardness, wear resistance, and heat resistance. The die insert experiences the highest pressure, so I selected YG20 cemented carbide for the insert. The middle ring and outer ring are made of H13 and 42CrMo, respectively. The material properties are summarized in Table 2. The cemented carbide has high compressive strength but relatively low tensile strength, so the die design must minimize tensile stress in the insert.

Die component Material Tensile strength (MPa) Elastic modulus (GPa) Poisson’s ratio
Insert YG20 220 580 0.22
Middle ring H13 654 210 0.30
Outer ring 42CrMo 980 209 0.30

3. Finite Element Modeling

I used a rigid-plastic finite element formulation because the billet undergoes large plastic deformation during cold extrusion. The elastic deformation of the billet can be neglected compared with the plastic deformation. The rigid-plastic finite element method is based on the Markov variational principle. The functional can be written as

$$
\phi = \int_V E(\dot{\bar{\varepsilon}}) \, dV – \int_{S_p} q_i v_i \, ds
$$

where \(E(\dot{\bar{\varepsilon}})\) is the power function, \(q_i\) are the prescribed surface tractions, \(v_i\) are the velocity components, and \(S_p\) is the traction boundary. To enforce volume constancy, I introduced a penalty term with a large positive number \(a\). The modified functional becomes

$$
\phi = \int_V E(\dot{\bar{\varepsilon}}) \, dV – \int_{S_p} q_i v_i \, ds + \frac{a}{2} \int_V (\dot{\varepsilon}_V)^2 \, dV
$$

where \(\dot{\varepsilon}_V\) is the volumetric strain rate. Taking the variation with respect to the velocity field and discretizing the domain leads to a set of nonlinear equations. Using the Newton-Raphson method, I solved the equations iteratively:

$$
\begin{cases}
\Delta \mu_n = N^{-1}(M – M_n) \\
\mu_{n+1} = \mu_n + \Delta \mu_n
\end{cases}
$$

I established a three-dimensional model of the gear, the billet, the upper punch, the lower punch, and the die. To save computation time, I used a one-tooth sector model with symmetry boundary conditions. The billet was defined as a plastic body, while the dies were treated as rigid bodies during the forming simulation. The mesh of the billet contained about 32,000 elements. The minimum element length was 0.663 mm, and the step size was set to 0.22 mm, which is about one third of the minimum element length.

Simulation parameter Value
Billet material 20CrMnTi
Billet mesh elements 32,000
Minimum element length 0.663 mm
Step size 0.22 mm
Temperature 20 °C
Upper punch velocity 20 mm/s
Friction coefficient 0.12
Boundary condition Symmetry plane
Volume compensation Active in FEM + meshing

The simulation showed that the tooth cavities filled completely and the forged gear blank had good shape quality. The forming load increased rapidly at the beginning, then reached a stable stage after the billet passed through the die forming zone and the lower punch land. The stable forming load was about 6,500 kN. This value was used as the basis for die design and press selection.

4. Theoretical Design of the Combined Die

The die insert is essentially a thick-walled cylinder subjected to internal pressure. I used the thick-walled cylinder theory and the Lamé equations to derive the relationship between the internal pressure and the diameter ratio. For a cylinder with inner radius \(r_1\) and outer radius \(r_i\), the radial and tangential stresses under internal pressure \(p_1\) and external pressure \(p_i\) can be written as

$$
\begin{cases}
\sigma_r = A – \frac{B}{r^2} \\
\sigma_\theta = A + \frac{B}{r^2}
\end{cases}
$$

where

$$
\begin{cases}
A = \frac{r_1^2 p_1 – r_i^2 p_i}{r_i^2 – r_1^2} \\
B = \frac{(p_1 – p_i) r_1^2 r_i^2}{r_i^2 – r_1^2}
\end{cases}
$$

According to the Tresca yield criterion, yielding occurs when the maximum shear stress reaches half of the yield strength:

$$
\tau_{\max} = \frac{1}{2}(\sigma_{\max} – \sigma_{\min}) = \frac{\sigma_s}{2}
$$

For a single-layer die, the maximum internal pressure that the die can withstand before yielding is

$$
p_{1\max} = \frac{1}{2}\left(1 – \frac{1}{n^2}\right)\sigma_s
$$

where \(n = r_2/r_1\) is the diameter ratio. For a two-layer combined die, the maximum internal pressure is

$$
p_{1\max} = \frac{1}{2}\left(1 – \frac{1}{n_2^2}\right)\sigma_{s2} + \frac{1}{2}\left(1 – \frac{1}{n_1^2}\right)\sigma_{s1}
$$

For a three-layer combined die, the maximum internal pressure is

$$
p_{1\max} = \frac{1}{2}\left(1 – \frac{1}{n_3^2}\right)\sigma_{s3} + \frac{1}{2}\left(1 – \frac{1}{n_2^2}\right)\sigma_{s2} + \frac{1}{2}\left(1 – \frac{1}{n_1^2}\right)\sigma_{s1}
$$

Using the Lagrange multiplier method, I obtained the optimal diameter ratios that maximize the load-carrying capacity:

$$
\begin{cases}
n_1 = \sqrt{\frac{\sigma_{s1}}{\sigma}} \\
n_2 = \sqrt{\frac{\sigma_{s2}}{\sigma}} \\
n_3 = \sqrt{\frac{\sigma_{s3}}{\sigma}}
\end{cases}
$$

where

$$
\sigma = \sqrt[3]{\frac{\sigma_{s1}\sigma_{s2}\sigma_{s3}}{n^2}}
$$

Based on the stable forming load, the internal pressure on the die insert was estimated to be about 1,154 MPa. Using the material strengths of the insert, middle ring, and outer ring, I calculated the total diameter ratio. A value of \(n = 4.7\) was selected to balance safety and cost. The resulting outer diameters were \(d_2 = 120\) mm, \(d_3 = 220\) mm, and \(d_4 = 350\) mm. The interference coefficients were initially set to \(\beta_2 = 2.5 \times 10^{-3}\) and \(\beta_3 = 3.0 \times 10^{-3}\). The corresponding single-side interferences were \(U_2 = 0.15\) mm and \(U_3 = 0.33\) mm.

Parameter Theoretical value
Insert inner diameter, d1 73.8 mm
Insert outer diameter, d2 120 mm
Middle ring outer diameter, d3 220 mm
Outer ring outer diameter, d4 350 mm
Total diameter ratio, n 4.7
Interference coefficient β2 2.5 × 10⁻³
Interference coefficient β3 3.0 × 10⁻³
Single-side interference U2 0.15 mm
Single-side interference U3 0.33 mm

5. Die Failure Analysis and New Die Structure

I first simulated the integral combined die. The tangential stress and axial stress distributions showed that the maximum tangential tensile stress reached about 630 MPa, which is much higher than the tensile strength of the cemented carbide insert. The maximum axial tensile stress was about 278 MPa. Increasing the interference coefficients to \(\beta_2 = 4 \times 10^{-3}\) and \(\beta_3 = 4 \times 10^{-3}\) reduced the tangential stress, but the axial tensile stress remained high. This indicated that the integral die was prone to cracking and fracture, especially in the axial direction.

Die type Maximum tangential stress Maximum axial stress Failure risk
Integral die, β2 = 2.5‰, β3 = 3‰ 630 MPa 278 MPa Very high
Integral die, β2 = 4‰, β3 = 4‰ Reduced Still high High

To reduce the axial tensile stress, I proposed a transverse split die. In this design, the die insert is split horizontally above the tooth forming zone. The split position is usually placed 1 to 2 mm above the center of the transition fillet. I chose 1.5 mm above the fillet center. The contact width between the split insert and the die was set to \(k = 1.8\) mm, and the slope behind the contact surface was 2 degrees. The transverse split die significantly reduced the axial tensile stress. However, during simulation I observed that the billet metal flowed into the gap between the insert and the die, creating a drilling defect. This defect would make the forged gear blank unacceptable.

The drilling defect occurred because the split upper and lower parts were fastened by bolts. The bolt preload and the axial preload acted at distant locations, creating a bending moment. This bending moment opened a gap between the insert and the die, and the billet metal was forced into the gap under high pressure. To solve this problem, I designed an axial-preloaded split die. In this structure, only the die insert is split transversely, and the prestress rings are not split. A nut is used at the bottom of the die insert to apply an axial preload. This design avoids the bending moment that occurs in the transverse split die and prevents the gap from opening.

I used the finite element method to determine the required axial preload. The axial preload was applied as a force on the bottom of the die insert. The contact width between the insert and the die was varied to study its effect. When the contact width was too large, the unit preload was too small, and drilling occurred. When the preload was too large, the die insert was pressed down or damaged. The simulation results showed that a contact width of \(k = 2\) mm and an axial force of \(F = 65,000\) N produced a unit preload of \(p = 2,237\) N/mm². At this condition, no drilling occurred, and the die stress remained below the material limits.

Axial force F (N) Unit preload p (N/mm²) Drilling condition
54,000 1,906 Severe drilling
56,000 1,977 Visible drilling
58,000 2,047 Drilling improved
61,000 2,153 Slight drilling
64,000 2,259 No drilling
67,000 2,365 No drilling, risk of damage

The contact width also influenced the drilling behavior. For a given axial force, a larger contact width reduced the unit preload and increased the gap. A smaller contact width increased the unit preload but could cause die damage if the force was too high. The results are summarized in Table 6. Based on these results, I selected \(k = 2\) mm and \(F = 65,000\) N for the axial-preloaded split die.

Contact width k (mm) Recommended axial force range (N) Observed behavior
1.0 60,000–65,000 Good, but high damage risk
1.5 62,000–67,000 Good
2.0 63,000–67,500 Best compromise
2.5 64,000–68,000 Slight drilling at low force
3.0 66,000–69,000 More drilling
3.5 68,000–70,000 Severe drilling at low force
4.0 70,000–72,000 Not recommended

6. Response Surface Optimization of the Axial-Preloaded Split Die

The theoretical dimensions provided a safe starting point, but they did not guarantee optimal use of the die materials. I therefore used the response surface method to optimize the die structure. The design variables were the interference coefficient \(\beta_2\), the interference coefficient \(\beta_3\), and the radial ratios \(n_{21} = d_2/d_1\), \(n_{31} = d_3/d_1\), and \(n_{41} = d_4/d_1\). The optimization objectives were the tangential stress in the insert, the tangential stress in the middle ring, and the tangential stress in the outer ring. I used a central composite design with five factors and five levels, resulting in 50 simulation runs.

Symbol Parameter Level -2 Level -1 Level 0 Level 1 Level 2
x1 β2 2.0 2.5 3.0 3.5 4.0
x2 β3 2.0 2.5 3.0 3.5 4.0
x3 n2 1.55 1.60 1.65 1.70 1.75
x4 n3 2.3 2.5 2.7 2.9 3.1
x5 n4 3.5 4.0 4.5 5.0 5.5

The regression models for the three responses were fitted as second-order polynomials. The general form is

$$
y = \beta_0 + \sum_{i=1}^{m} \beta_i x_i + \sum_{i=1}^{m} \beta_{ii} x_i^2 + \sum_{i<j} $$="" +=""

For the insert tangential stress \(y_1\), the fitted model was

$$
\begin{aligned}
y_1 = & -2190.8912 – 22.80187x_1 – 2.71125x_2 + 2482.23438x_3 + 317.4x_4 + 7.08375x_5 \\
& + 1.81875x_1x_2 + 3x_1x_3 + 3.78125x_1x_4 + 3.56875x_1x_5 – 11.375x_2x_3 \\
& + 10.59375x_2x_4 + 1.36875x_2x_5 – 22.03125x_3x_4 – 53.75x_3x_5 + 8.71875x_4x_5 \\
& – 7.39625x_1^2 – 5.48375x_2^2 – 735.875x_3^2 – 70.05469x_4^2 + 3.64125x_5^2
\end{aligned}
$$

For the middle ring tangential stress \(y_2\), the fitted model was

$$
\begin{aligned}
y_2 = & -342.04783 – 99.12187x_1 – 36.79656x_2 + 2336.99688x_3 – 256.92031x_4 – 91.33062x_5 \\
& + 1.7125x_1x_2 + 110.5x_1x_3 – 4.5x_1x_4 – 1.46875x_1x_5 + 9.43750x_2x_3 \\
& + 21.01562x_2x_4 + 8.75x_2x_5 – 35.46875x_3x_4 + 6.25x_3x_5 + 23.34375x_4x_5 \\
& – 9.16375x_1^2 – 16.66375x_2^2 – 852.625x_3^2 + 23.74219x_4^2 – 4.03875x_5^2
\end{aligned}
$$

For the outer ring tangential stress \(y_3\), the fitted model was

$$
\begin{aligned}
y_3 = & 6422.38505 + 256.62687x_1 + 169.31281x_2 – 5316.64063x_3 – 836.07656x_4 – 523.08375x_5 \\
& – 1.2375x_1x_2 – 153.875x_1x_3 – 10x_1x_4 + 12.65625x_1x_5 – 0.43750x_2x_3 \\
& + 1.85938x_2x_4 + 1.5125x_2x_5 + 187.65625x_3x_4 + 125.375x_3x_5 – 6.6875x_4x_5 \\
& – 8.35875x_1^2 – 17.57125x_2^2 + 1489.125x_3^2 + 110.17969x_4^2 + 33.86625x_5^2
\end{aligned}
$$

The analysis of variance showed that the models were highly significant. The F values for \(y_1\), \(y_2\), and \(y_3\) were 15.69, 24.93, and 8.59, respectively, and the P values were all 0.0001. The coefficients of determination \(R^2\) were 0.9154, 0.9450, and 0.9276, and the adjusted \(R^2\) values were 0.8570, 0.9071, and 0.8777. These values indicate that the response surface models fit the simulation data well and can be used for optimization.

Response F value P value R² Adjusted R² Adequate precision
y1 (insert tangential stress) 15.69 0.0001 0.9154 0.8570 15.466
y2 (middle ring tangential stress) 24.93 0.0001 0.9450 0.9071 22.293
y3 (outer ring tangential stress) 8.59 0.0001 0.9276 0.8777 20.643

The optimization was carried out with the constraints that the stresses in the insert, middle ring, and outer ring should remain below the tensile strength of their respective materials. The optimal parameter combination was found to be \(\beta_2 = 4.0 \times 10^{-3}\), \(\beta_3 = 2.5 \times 10^{-3}\), \(n_2 = 1.74\), \(n_3 = 3.09\), and \(n_4 = 4.78\). The corresponding dimensions were \(d_2 = 130\) mm, \(d_3 = 230\) mm, and \(d_4 = 360\) mm. The single-side interferences were \(U_1 = 0.26\) mm and \(U_2 = 0.29\) mm. These optimized dimensions were slightly larger than the theoretical values, but they ensured that the die stresses stayed within safe limits.

Design method d2 (mm) d3 (mm) d4 (mm) U1 (mm) U2 (mm)
Theoretical design 120 220 350 0.15 0.33
Optimized design 130 230 360 0.26 0.29

I simulated the optimized die and compared the stresses with the theoretical design. The optimized insert stress was -113.8 MPa, the middle ring stress was 569.6 MPa, and the outer ring stress was 648.3 MPa. All values were below the material limits. The deviations between the predicted and optimized values were small, which confirmed the accuracy of the response surface optimization.

Response Predicted (MPa) Theoretical (MPa) Optimized (MPa) Deviation from prediction Deviation from theory
Insert stress -121.9 -101 -113.8 5.7% 11.2%
Middle ring stress 539.7 619 569.6 5.4% 8.7%
Outer ring stress 619.6 673 648.3 4.4% 3.8%

7. Effects of Process Parameters on Gear Forming and Die Stress

After the die structure was optimized, I studied how the die process parameters affect the forming quality of the forged gear blank and the stress in the die. The parameters included the entry half angle \(\alpha\), the root width \(T\) at the die entry, and the friction coefficient \(\mu\). These parameters directly influence metal flow, forming load, and die stress.

7.1 Entry Half Angle

The entry half angle is the angle between the die entry surface and the extrusion axis. I simulated values of 25°, 30°, 35°, 40°, 45°, 50°, 55°, 60°, 65°, 70°, and 75°. The results showed that as the entry half angle increased, the sag length at the lower end of the gear decreased. For example, at 25°, the sag length was 3.08 mm, while at 55°, it was 1.31 mm. However, the forming load increased with the entry half angle. The stable load increased slowly from 25° to 60°, but increased rapidly above 60°. The maximum equivalent stress in the die insert also increased with the entry half angle. A larger angle increased the deformation zone and the resistance to metal flow, requiring higher pressure. Considering both forming quality and die stress, I selected an entry half angle of 60°.

Entry half angle α Sag length (mm) Stable load trend Die stress trend
25° 3.08 Low Low
35° 2.45 Moderate Moderate
45° 1.82 Moderate Moderate
55° 1.31 Higher Higher
60° 1.20 High High
65° 1.15 Rapid increase Rapid increase
75° 1.10 Very high Very high

7.2 Root Width at the Die Entry

The root width \(T\) at the die entry acts as a flow divider. I simulated values of 0.8, 1.6, 2.4, 3.2, 4.0, 4.8, 5.6, and 6.2 mm. The sag length increased with increasing root width. When the root width was between 0.8 and 4.8 mm, the sag length increased gradually. Above 4.8 mm, the sag length increased rapidly. The stable forming load and the die stress also increased with the root width. A wider root increases the plastic deformation zone and the resistance to axial flow. However, if the root width is too small, the die entry becomes too sharp and can damage the phosphate coating on the billet, leading to sticking. Therefore, I selected a root width of 3.2 mm.

Root width T (mm) Sag length trend Forming load trend Die stress trend
0.8 Small Low Low
1.6 Small Low Low
2.4 Moderate Moderate Moderate
3.2 Moderate Moderate Moderate
4.0 Larger Higher Higher
4.8 Larger Higher Higher
5.6 Rapid increase High High
6.2 Very large Very high Very high

7.3 Friction Coefficient

Friction is unavoidable in cold extrusion. I simulated friction coefficients of 0.04, 0.08, 0.12, 0.16, and 0.22. The forming load increased with the friction coefficient. The stable load at \(\mu = 0.22\) was much higher than at \(\mu = 0.04\). The maximum equivalent stress in the die insert also increased with friction. When the friction coefficient exceeded 0.12, the stress increased more rapidly. High friction can damage the billet surface, break the lubricating film, and cause sticking. Therefore, reducing friction through good lubrication and smooth die surfaces is essential for producing a high-quality forged gear blank and avoiding die failure.

Friction coefficient μ Stable load trend Die stress trend Surface quality risk
0.04 Lowest Lowest Low
0.08 Low Low Low
0.12 Moderate Moderate Moderate
0.16 High High High
0.22 Very high Very high Very high

8. Experimental Verification and Industrial Application

I designed and manufactured a trial die based on the optimized axial-preloaded split die structure. The key parameters are listed in Table 12. The die insert was made of YG20 cemented carbide, the middle ring of H13, and the outer ring of 42CrMo. The insert cavity was machined by slow-wire electrical discharge machining, followed by electrical discharge machining for the complex entry region and polishing. The die was assembled with the axial preload applied by a nut at the bottom of the insert.

Process parameter Value
Outer ring outer diameter, d4 360 mm
Middle ring outer diameter, d3 230 mm
Insert outer diameter, d2 130 mm
Single-side interference U1 0.26 mm
Single-side interference U2 0.29 mm
Entry half angle α 60°
Root width T 3.2 mm
Contact width k 2.0 mm
Axial preload F 65,000 N

The billet was prepared from a 20CrMnTi hot-rolled bar with a diameter of 85 mm. The bar was sawn to a length of 36 mm. I annealed the billet to reduce hardness and improve plasticity. The annealed microstructure consisted of ferrite and pearlite, with a hardness of 120–140 HBS. The billet was then turned to remove surface defects and oxide scale. Before extrusion, the billet was phosphated and saponified to form a lubricating film. This treatment reduces friction and prevents direct metal-to-metal contact between the billet and the die cavity.

The extrusion trial was carried out on an 8,000 kN frame hydraulic press. The upper punch moved downward at a controlled speed, while the lower punch remained fixed. The forged gear blank was formed in one stroke. After extrusion, the upper punch retracted, and the ejector pushed the forged gear blank out of the die cavity. The trial results showed that the tooth cavities were completely filled, and no drilling defect occurred. The measured forming load was 5,960 kN, which was about 9.1% lower than the simulated value of 6,500 kN. This difference is acceptable and confirms the reliability of the finite element model.

The forged gear blank obtained from the axial-preloaded split die is shown below.

After the trial, the die was put into production. The axial-preloaded split die has been used to produce more than 50,000 pieces. The die insert showed no cracks, fractures, or other failure modes. The common normal length of the forged gear blank was measured periodically. After 50,000 pieces, the common normal length was in the range of 32.32–32.34 mm, which is within the design requirement of 32.30 +0.06 mm. The die life is expected to exceed 100,000 pieces. This confirms that the axial-preloaded split die structure is feasible and effective for industrial production.

Production quantity Common normal length (mm) Die condition
First piece 32.30–32.32 Good
25,000 pieces 32.31–32.33 Good
50,000 pieces 32.32–32.34 Good, no cracks

9. Conclusions

I have developed a complete design method for cold extrusion dies used to produce a straight-tooth cylindrical gear. The main conclusions are as follows.

First, the integral combined die experiences high tangential and axial tensile stresses. Increasing the interference reduces the tangential stress but has little effect on the axial stress. The axial tensile stress can cause cracking and fracture, so the integral die is not suitable for this application.

Second, the transverse split die reduces the axial tensile stress, but it creates a gap between the insert and the die because the bolt preload and the axial preload act at different locations. This gap causes billet metal to flow into the gap, creating a drilling defect. The axial-preloaded split die solves this problem by splitting only the insert and applying an axial preload with a nut at the bottom. The optimal axial preload is \(F = 65,000\) N with a contact width of \(k = 2\) mm, giving a unit preload of \(p = 2,237\) N/mm².

Third, the response surface method successfully optimized the die structure. The optimal dimensions are \(d_2 = 130\) mm, \(d_3 = 230\) mm, \(d_4 = 360\) mm, \(U_1 = 0.26\) mm, and \(U_2 = 0.29\) mm. The optimized die keeps the stresses in all rings below their material limits and uses the die materials more efficiently.

Fourth, the entry half angle, root width, and friction coefficient significantly affect the forming quality and die stress. I selected an entry half angle of 60°, a root width of 3.2 mm, and recommended low friction through good lubrication. These parameters help produce a well-filled forged gear blank while keeping the die stress within safe limits.

Fifth, the industrial trial confirmed the feasibility of the axial-preloaded split die. The forged gear blank had complete tooth filling and no drilling defect. The die produced more than 50,000 pieces without failure, and the common normal length remained within the design requirement. The experimental forming load was 5,960 kN, which is 9.1% lower than the simulated value. The results validate both the die design method and the finite element simulation.

Overall, my research shows that the axial-preloaded split die structure can effectively prevent early die failure and support the industrial application of cold extrusion for producing a high-quality forged gear blank. This work provides a practical design method for gear cold extrusion dies and contributes to the wider use of cold extrusion in gear manufacturing.

Scroll to Top