Cold Extrusion Die Design for Gears

I investigated the cold extrusion of a heavy-truck planetary spur gear and focused on the failure modes of the cold extrusion die and on a design method that can suppress those failure modes. The target part is a straight cylindrical gear with external teeth and a central bore. I treated the process as a forward cold extrusion operation in which an upper punch moves downward, a lower punch remains fixed, the external tooth profile is formed by the die cavity, and the bore is formed by the lower punch. The resulting forged gear blanks require only limited machining after extrusion. My main objective was to explain why the die fails under the very high forming load and to develop a die structure that keeps the die core in compression, prevents metal drilling into die gaps, and provides a robust basis for industrial production of forged gear blanks.

Part Characteristics and Process Scheme

I first analyzed the geometry of the target gear. The gear has 18 teeth, module 4.1 mm, pressure angle 22.5 degrees, and a positive addendum modification. The external tip diameter is 83.09 mm, the root diameter is 67.37 mm, and the bore diameter is 44.95 mm. The material is 20CrMnTi, which has good cold formability and is suitable for cold extrusion of forged gear blanks. The main geometric parameters are summarized in Table 1.

Parameter Symbol Value Unit
Module m 4.1 mm
Number of teeth z 18 –
Pressure angle alpha 22.5 degree
Addendum modification coefficient x 0.366 –
Tip diameter d_a 83.09 mm
Root diameter d_f 67.37 mm
Bore diameter d_i 44.95 mm
Blank material – 20CrMnTi –

I adopted a forward extrusion scheme because it allows the external teeth and the bore to be formed in one press stroke. The upper punch moves at a controlled speed, the lower punch supports the blank and forms the bore, and the formed gear is ejected by a knockout rod. This scheme shortens the process chain and improves material utilization. However, the forming force is large, and the die core is the principal load-bearing component. If the die core experiences excessive tensile stress, cracks, fracture, or local plastic deformation can occur. These failure modes interrupt production and increase the cost of forged gear blanks.

Die Materials and Finite Element Model

I used a three-layer prestressed die structure. The die core was made of YG20 cemented carbide, the middle prestressing ring of H13 hot-work die steel, and the outer ring of 42CrMo. The material properties are listed in Table 2. The core material has high hardness and wear resistance but low tensile strength, so the design must keep the core in compression as much as possible. The prestressing rings were used to generate a compressive preload on the core and to reduce the tangential tensile stress during extrusion.

Die layer Material Tensile strength (MPa) Elastic modulus (GPa) Poisson ratio
Core YG20 220 580 0.22
Middle ring H13 654 210 0.30
Outer ring 42CrMo 980 209 0.30

I built the finite element model in a commercial forming simulation environment. To reduce computation time, I used a one-tooth sector corresponding to 1/18 of the gear. The blank was treated as a rigid-plastic body, while the dies were treated as elastic bodies for die stress analysis. The flow stress of 20CrMnTi was taken from the material database. The main simulation settings are summarized in Table 3. The rigid-plastic formulation with a penalty term can be written as

$$ \Phi = \int_V E(\dot{\bar{\varepsilon}})\,dV – \int_{S_p} q_i v_i\,ds + \frac{\alpha}{2}\int_V (\dot{\varepsilon}_v)^2\,dV $$

where \(E(\dot{\bar{\varepsilon}})\) is the power function, \(q_i\) is the prescribed traction, \(v_i\) is the velocity, \(\dot{\varepsilon}_v\) is the volumetric strain rate, and \(\alpha\) is a large penalty factor. The variation of this functional leads to the discretized equilibrium equations used by the solver. I used a Newton-Raphson iteration scheme and a relaxation solver. The volume compensation option was activated during remeshing to reduce volume loss in the highly deformed forged gear blanks.

Parameter Setting
Model type One-tooth sector, 1/18 of full gear
Blank mesh count 32,000 elements
Minimum element size 0.663 mm
Step size 0.22 mm
Punch speed 20 mm/s
Initial temperature 20 degrees C
Friction coefficient 0.12
Volume compensation Active during remeshing
Solver Relaxation solver with Newton-Raphson iteration

The simulated forming process showed that the tooth cavities filled completely and that the forged gear blanks had a sound external profile. The forming load increased rapidly during the initial filling stage, then reached a stable plateau after the blank passed the die entrance and the lower punch land. The stable forming load was about 6,500 kN, which was used as the basis for die stress analysis and press selection.

Theoretical Sizing of the Prestressed Die

I treated each die ring as a thick-walled cylinder under internal and external pressure. For a cylinder with inner radius \(r_1\), outer radius \(r_i\), internal pressure \(p_1\), and external pressure \(p_i\), the radial and tangential stresses are

$$ \sigma_r = A – \frac{B}{r^2}, \qquad \sigma_\theta = A + \frac{B}{r^2} $$

with

$$ A = \frac{r_1^2 p_1 – r_i^2 p_i}{r_i^2 – r_1^2}, \qquad B = \frac{(p_1 – p_i)r_1^2 r_i^2}{r_i^2 – r_1^2} $$

According to the Tresca yield criterion, yielding begins when the maximum shear stress reaches the shear yield strength:

$$ \tau_{\max} = \frac{\sigma_\theta – \sigma_r}{2} = \frac{\sigma_s}{2} \qquad \text{or} \qquad \sigma_\theta – \sigma_r = \sigma_s $$

For a single thick-walled cylinder with external pressure equal to zero and diameter ratio \(n = r_i/r_1\), the maximum internal pressure that can be carried before yielding is

$$ p_{1\max} = \frac{1}{2}\left(1 – \frac{1}{n^2}\right)\sigma_s $$

For a two-layer die, the maximum internal pressure can be expressed as

$$ p_1 = \frac{1}{2}\left(1 – \frac{1}{n_2^2}\right)\sigma_{s2} + \frac{1}{2}\left(1 – \frac{1}{n_1^2}\right)\sigma_{s1} $$

For a three-layer die, the corresponding expression is

$$ p_1 = \frac{1}{2}\left(1 – \frac{1}{n_3^2}\right)\sigma_{s3} + \frac{1}{2}\left(1 – \frac{1}{n_2^2}\right)\sigma_{s2} + \frac{1}{2}\left(1 – \frac{1}{n_1^2}\right)\sigma_{s1} $$

Using the Lagrange multiplier method under the condition \(n = n_1 n_2 n_3\), the optimum diameter ratios for a three-layer die are

$$ n_1 = \sqrt{\frac{\sigma_{s1}}{\sigma}}, \qquad n_2 = \sqrt{\frac{\sigma_{s2}}{\sigma}}, \qquad n_3 = \sqrt{\frac{\sigma_{s3}}{\sigma}} $$

where

$$ \sigma = \sqrt[3]{\frac{\sigma_{s1}\sigma_{s2}\sigma_{s3}}{n^2}} $$

The total diameter ratio can be estimated from

$$ n = \sqrt[3]{\frac{\sigma_{s1}\sigma_{s2}\sigma_{s3}}{\left[\frac{1}{3}\left(\sigma_{s1}+\sigma_{s2}+\sigma_{s3}\right)-\frac{2}{3}p_1\right]^3}} $$

I used the simulated internal pressure of about 1,154 MPa and the material strengths listed in Table 2. The calculation gave \(n=4.4\). To provide a safety margin, I selected a total diameter ratio \(n=4.7\). With the die core inner diameter \(d_1=73.8\) mm, the theoretical outer diameter was \(d_4=350\) mm. The intermediate diameters were \(d_2=120\) mm and \(d_3=220\) mm. The interference coefficients were selected as \(\beta_2=2.5\times 10^{-3}\) and \(\beta_3=3.0\times 10^{-3}\), giving unilateral interferences of 0.15 mm and 0.33 mm. These values are listed in Table 4.

Parameter Theoretical value Unit
Core inner diameter \(d_1\) 73.8 mm
Core outer diameter \(d_2\) 120 mm
Middle ring outer diameter \(d_3\) 220 mm
Outer ring outer diameter \(d_4\) 350 mm
Interference coefficient \(\beta_2\) 2.5 x 10^-3 –
Interference coefficient \(\beta_3\) 3.0 x 10^-3 –
Unilateral interference \(U_1\) 0.15 mm
Unilateral interference \(U_2\) 0.33 mm

For die stress analysis, I mapped the stable forming load from the extrusion simulation onto the inner surface of the die core by interpolation. The core was discretized with about 50,000 elements, and each prestressing ring with about 32,000 elements. This procedure allowed me to evaluate the stress state of the die under the actual forming load without repeating the full coupled simulation for every die variant.

Failure Analysis of the Integral Die

The integral three-layer die was analyzed first. Under the stable forming load, the core exhibited a large tangential tensile stress near the tooth entrance. The maximum tangential tensile stress reached about 630 MPa, which is far above the tensile strength of the cemented carbide core. A significant axial tensile stress of about 278 MPa also appeared above the tooth entrance. These stresses are summarized in Table 5. Because cemented carbide has low tensile strength, the integral die is prone to cracking, chipping, and fracture. Increasing the interference of the prestressing rings reduced the tangential stress, but it had little effect on the axial tensile stress. Therefore, the integral die could not be made sufficiently reliable only by increasing the radial preload.

Die type Interference condition Max tangential stress (MPa) Max axial stress (MPa) Observed risk
Integral die \(\beta_2=2.5\times10^{-3}\), \(\beta_3=3.0\times10^{-3}\) 630 278 Core cracking and fracture
Integral die \(\beta_2=4.0\times10^{-3}\), \(\beta_3=4.0\times10^{-3}\) Reduced Still high Axial tensile cracking

The dominant failure modes I identified were low-cycle fatigue cracking, abrasive wear, local plastic deformation, and brittle fracture of the core. The stress state can be interpreted with the Tresca criterion and with a simple fatigue damage accumulation rule. If the equivalent stress range is \(\Delta\sigma\), the fatigue damage per cycle can be written as

$$ D = \sum_{i=1}^{N}\left(\frac{\Delta\sigma_i}{\sigma_f}\right)^m $$

where \(\sigma_f\) is a fatigue strength parameter and \(m\) is a material exponent. Because the die is repeatedly loaded and unloaded, even a moderate stress amplitude can lead to fatigue crack initiation at the tooth entrance. The tensile axial stress is especially dangerous because it acts on the brittle carbide core. Therefore, I concluded that the die structure should be changed so that the axial tensile stress is reduced or eliminated.

Transverse Split Die and the Drilling Problem

I then examined a transverse split die structure. The integral die core was split horizontally above the tooth forming zone. The split position was selected about 1.5 mm above the center of the transition fillet. The contact width between the die insert and the die core was \(k=1.8\) mm, and the mating surface behind the contact area was inclined at 2 degrees. The prestressing rings were split at the same height as the core, and the upper and lower parts were fastened by bolts. The stress analysis showed that the transverse split significantly reduced the axial tensile stress in the core. Increasing the interference also reduced the tangential stress. However, during the extrusion simulation, the blank metal flowed into the gap between the split insert and the core, producing a severe drilling defect. This defect is unacceptable because it damages the die and produces incomplete forged gear blanks.

The drilling was caused by the separation of the mating surfaces under the axial forming load. The bolted preload acted at a position far from the contact interface, so the preload generated a bending moment. This bending moment opened a gap between the die insert and the core. Once the gap appeared, the highly pressurized blank metal entered the gap. I expressed the contact pressure as

$$ p_c = \frac{F}{A_c} $$

where \(F\) is the axial preload and \(A_c\) is the contact area. For a narrow contact band, \(A_c = k l_c\), where \(k\) is the contact width and \(l_c\) is the contact length. Reducing \(k\) increases the contact pressure for a given force, but it also increases the risk of local crushing. Increasing \(k\) reduces the contact pressure and allows the gap to open. Therefore, a transverse split die with a remote bolt preload cannot simultaneously guarantee sufficient contact pressure and avoid bending deformation. I confirmed this limitation by comparing the transverse split die with the same axial preload applied to a modified core and observing continued drilling in the transverse split configuration.

Axially Preloaded Split Die

To eliminate the drilling defect while retaining the benefit of the split core, I proposed an axially preloaded split die. In this design, only the die core is split horizontally. The prestressing rings remain continuous and unsplit. The split core is clamped in the axial direction by a nut at the bottom of the die. The axial preload is applied directly near the split interface, so the bending moment that caused the gap in the transverse split die is avoided. The die insert sits on the split core, and the contact width \(k\) is kept small enough to generate a high contact pressure. The mating surface behind the contact band has a small slope, which helps to maintain contact during loading. This structure is intended to keep the core in compression, reduce the axial tensile stress, and prevent blank metal from entering the split interface.

I simulated the axial preload by applying a concentrated axial force to the die core in the finite element model. The force \(F\) was varied from 54,000 N to 67,000 N. The corresponding contact pressures were calculated from \(p=F/A_c\). The results are summarized in Table 6. At \(F=54,000\) N, the gap was still open and drilling occurred. At \(F=58,000\) N, the drilling was significantly reduced. At \(F=64,000\) N, no drilling was observed. When \(F\) exceeded about 67,000 N, the die insert began to move downward or the contact region was locally crushed, indicating that the preload was excessive. Therefore, the axial preload must be selected within a window that is high enough to close the gap but low enough to avoid die damage.

Axial force \(F\) (N) Contact pressure \(p\) (N/mm^2) Observed condition
54,000 1,906 Visible drilling
56,000 1,977 Reduced drilling
58,000 2,047 Drilling significantly reduced
61,000 2,153 Minor drilling tendency
64,000 2,259 No drilling
67,000 2,365 No drilling but risk of crushing

I also studied the influence of the contact width \(k\). Seven values were considered: 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, and 4.0 mm. For each width, the axial force was varied over the same range. The gap opening was measured as the separation between the die insert and the core during extrusion. A positive gap indicated drilling, while a negative value indicated downward movement of the insert. The results showed that a larger contact width reduced the contact pressure and promoted drilling. A very small contact width increased the risk of local crushing. The safe combination was found near \(k=2.0\) mm and \(F=65,000\) N, corresponding to \(p=2,237\) N/mm^2. Under this condition, the split interface remained closed, no drilling occurred, and the core stress remained compressive. This design was therefore selected for further optimization of the die dimensions.

Response Surface Optimization of the Die Structure

The theoretical die dimensions provided a safe starting point, but they did not guarantee that the material capacity of each ring was fully utilized. I therefore used a response surface methodology to optimize the die structure. The design variables were the interference coefficient \(\beta_2\), the interference coefficient \(\beta_3\), and the radial diameter ratios \(n_{21}=d_2/d_1\), \(n_{31}=d_3/d_1\), and \(n_{41}=d_4/d_1\). The response targets were the maximum tangential stress in the core \(y_1\), the maximum tangential stress in the middle ring \(y_2\), and the maximum tangential stress in the outer ring \(y_3\). The goal was to keep all stresses below the allowable values while avoiding excessive tensile stress in the core and avoiding over-design. The design levels are listed in Table 7.

Variable Parameter Level -2 Level -1 Level 0 Level +1 Level +2
\(x_1\) \(\beta_2\) (x10^-3) 2.0 2.5 3.0 3.5 4.0
\(x_2\) \(\beta_3\) (x10^-3) 2.5 3.0 3.5 4.0 4.5
\(x_3\) \(n_{21}\) 1.55 1.60 1.65 1.70 1.75
\(x_4\) \(n_{31}\) 2.30 2.50 2.70 2.90 3.10
\(x_5\) \(n_{41}\) 3.50 4.00 4.50 5.00 5.50

I used a central composite design with five factors and five levels, giving 50 simulation runs. For each run, I built the die model, mapped the stable forming load, and extracted the three stress responses. A second-order polynomial response surface was fitted to the data. The general form is

$$ y = \beta_0 + \sum_{i=1}^{m}\beta_i x_i + \sum_{i=1}^{m}\beta_{ii}x_i^2 + \sum_{i<j}\beta_{ij}x_i $$="" +=""

The fitted regression models for the three responses were used for analysis and optimization. For example, the core stress model had the form

$$ \begin{aligned}
y_1 = {} & -2190.8912 – 22.80187x_1 – 2.71125x_2 + 2482.23438x_3 + 317.4x_4 + 7.08375x_5 \\
& + 1.81875x_1x_2 + 3x_1x_3 + 3.78125x_1x_4 + 3.56875x_1x_5 – 11.375x_2x_3 \\
& + 10.59375x_2x_4 + 1.36875x_2x_5 – 22.03125x_3x_4 – 53.75x_3x_5 + 8.71875x_4x_5 \\
& – 7.39625x_1^2 – 5.48375x_2^2 – 735.875x_3^2 – 70.05469x_4^2 + 3.64125x_5^2
\end{aligned} $$

The middle-ring and outer-ring models were constructed in the same manner. The analysis of variance showed that the models were highly significant. The probability values for all three models were below 0.01, and the coefficients of determination were 0.9154, 0.9450, and 0.9276 for \(y_1\), \(y_2\), and \(y_3\), respectively. The adjusted coefficients of determination were 0.8570, 0.9071, and 0.8777. The precision values were 15.466, 22.293, and 20.643, all well above the threshold of 4. These results are listed in Table 8. The models therefore provided an accurate representation of the relationship between the die dimensions and the die stresses.

Response model \(R^2\) Adjusted \(R^2\) Precision Model significance
Core stress \(y_1\) 0.9154 0.8570 15.466 Highly significant
Middle-ring stress \(y_2\) 0.9450 0.9071 22.293 Highly significant
Outer-ring stress \(y_3\) 0.9276 0.8777 20.643 Highly significant

The response surfaces showed that increasing the interference coefficient \(\beta_2\) increased the compressive stress in the core and reduced the risk of core cracking. Increasing the interference coefficient \(\beta_3\) reduced the stress in the middle ring but increased the stress in the outer ring. The radial ratios also had strong effects. A larger \(n_{21}\) reduced the stress in the middle ring, while a larger \(n_{41}\) reduced the stress in the outer ring up to a certain point and then increased it again. These trends allowed me to define a constrained optimization problem. The design variables were constrained within the ranges listed in Table 7. The response targets were constrained to keep the core in compression and to keep the ring stresses below the allowable values. The optimization ranges were

$$ -140\ \text{MPa} < y_1 < -120\ \text{MPa}, \qquad 450\ \text{MPa} < y_2 < 540\ \text{MPa}, \qquad 550\ \text{MPa} < y_3 < 620\ \text{MPa} $$

The optimum combination was \(\beta_2=4.0\times10^{-3}\), \(\beta_3=2.5\times10^{-3}\), \(n_{21}=1.74\), \(n_{31}=3.09\), and \(n_{41}=4.78\). The corresponding dimensions were \(d_2=130\) mm, \(d_3=230\) mm, and \(d_4=360\) mm. The unilateral interferences were \(U_1=0.26\) mm and \(U_2=0.29\) mm. I compared the theoretical and optimized dimensions in Table 9. The overall die size increased by only about 2.8 percent, but the stress distribution was improved and the material utilization was more balanced.

Design method \(d_2\) (mm) \(d_3\) (mm) \(d_4\) (mm) \(U_1\) (mm) \(U_2\) (mm)
Theoretical design 120 220 350 0.15 0.33
Optimized design 130 230 360 0.26 0.29

I validated the optimized design by rebuilding the die model and repeating the die stress analysis. The core remained in compression, and the tangential stresses in the middle and outer rings were below their tensile strengths. The predicted, theoretical, and optimized stress values are compared in Table 10. The optimized design increased the compressive stress in the core slightly, reduced the stress in the middle ring, and reduced the stress in the outer ring. All values were within the allowable limits, so the optimized die was adopted for process parameter studies and for the experimental die.

Case Core stress (MPa) Middle-ring stress (MPa) Outer-ring stress (MPa)
Response surface prediction -121.9 539.7 619.6
Theoretical design -101.0 619.0 673.0
Optimized design -113.8 569.6 648.3
Absolute deviation from prediction 5.7 percent 5.4 percent 4.4 percent
Absolute deviation from theoretical 11.2 percent 8.7 percent 3.8 percent

Effects of Die Process Parameters

After the die structure was fixed, I studied how the die entrance geometry and friction affect the forming quality, forming load, and die stress. The entrance half angle \(\alpha\), the tooth root width at the die entrance \(T\), and the friction coefficient \(\mu\) were selected because they directly influence metal flow into the tooth cavities and the pressure on the die core. These parameters are important for producing sound forged gear blanks with a long die life.

The entrance half angle was varied from 25 to 75 degrees. The collapse length at the lower end of the extruded gear decreased as the entrance angle increased. At 25 degrees, the collapse length was about 3.08 mm. At 55 degrees, it decreased to about 1.31 mm. Beyond 60 degrees, the decrease became gradual. The stable forming load increased with the entrance angle. The increase was moderate between 25 and 60 degrees and became steeper above 60 degrees. The maximum equivalent stress in the die core also increased with the entrance angle. A smaller angle reduced the load and die stress but increased the collapse length and the machining allowance. A larger angle improved the tooth-end quality but increased the risk of die failure. Considering both the forming quality of forged gear blanks and the die stress, I selected \(\alpha=60\) degrees. The trends are summarized in Table 11.

Entrance half angle \(\alpha\) (degree) Collapse length trend Stable load trend Core stress trend Assessment
25 Long, about 3.08 mm Low Low Good for die, poor for blank quality
35 Moderate Moderate Moderate Balanced but not optimal
55 Short, about 1.31 mm Moderate Moderate Good balance
60 Short Moderate to high Moderate to high Selected
75 Very short High High High die failure risk

The tooth root width at the die entrance was varied from 0.8 to 6.2 mm. A wider root width increased the collapse length and enlarged the plastic deformation zone. The stable forming load increased with the root width, and the increase became faster when the width exceeded about 4.8 mm. The maximum equivalent stress in the die core also increased with the root width. A very narrow root width, however, made the entrance edge too sharp. The sharp edge tended to damage the phosphate coating on the blank and could cause sticking between the blank and the die. Therefore, the root width must be wide enough to protect the lubrication layer but narrow enough to limit the forming load and die stress. I selected \(T=3.2\) mm. The trends are listed in Table 12.

Entrance root width \(T\) (mm) Collapse length trend Stable load trend Core stress trend Assessment
0.8 Short Low Low Sharp edge, risk of coating damage
1.6 Short Low to moderate Low to moderate Good but edge still sharp
3.2 Moderate Moderate Moderate Selected
4.8 Moderate to long Moderate to high Moderate to high Load increases faster
6.2 Long High High High die stress and material waste

The friction coefficient was varied from 0.04 to 0.22. Friction is unavoidable in cold extrusion, especially when producing forged gear blanks with a large contact area. A higher friction coefficient increased the forming load and the maximum equivalent stress in the die core. The increase was moderate between 0.04 and 0.12 and became steeper above 0.12. Excessive friction also increased the risk of surface tearing, coating breakdown, and sticking. Therefore, the die cavity should be polished, and the blank should be properly phosphated and saponified before extrusion. The friction results are summarized in Table 13.

Friction coefficient \(\mu\) Forming load trend Core stress trend Surface quality risk
0.04 Lowest Lowest Low
0.08 Low Low Low
0.12 Moderate Moderate Moderate
0.16 High High Coating damage possible
0.22 Highest Highest Sticking and tearing risk

Experimental Validation and Die Service Life

I designed and manufactured a production trial die using the optimized axially preloaded split die structure and the selected process parameters. The blank was cut from a 20CrMnTi hot-rolled bar of 85 mm diameter to a length of 36 mm. The blank was annealed to reduce hardness and improve cold formability. The annealed microstructure consisted of ferrite and pearlite, and the hardness was in the range of 120 to 140 HBS. The blank was then turned to remove the oxide scale and surface defects. Before extrusion, the blank was phosphated and saponified to form a lubricating film. The process flow was: bar sawing, annealing, turning, phosphating and saponification, cold extrusion, and inspection. The trial was performed on an 8,000 kN frame hydraulic press. The main press parameters are listed in Table 14.

Press parameter Value Unit
Nominal force 8,000 kN
Ejection force 1,500 kN
Maximum slider stroke 900 mm
Maximum hydraulic pressure 25 MPa
Pressing speed 13 to 31 mm/s
Return speed 150 mm/s
Total motor power 112 kW

The die core cavity was machined by slow wire electrical discharge machining to obtain the required tooth profile. The complex entrance transition and tooth fillet regions were finished by electrical discharge machining and then polished. The prestressing rings were machined with the optimized interference fits. The core was split horizontally, and the axial preload was applied by a nut at the bottom of the die. The contact width between the insert and the core was 2.0 mm, and the axial preload was set to 65,000 N, giving a contact pressure of about 2,237 N/mm^2.

The trial produced forged gear blanks with complete tooth filling and no drilling at the split interface. The measured forming force was 5,960 kN, while the simulated stable forming force was 6,500 kN. The difference was about 9.1 percent, which is acceptable for a cold extrusion process with complex friction and material behavior. The lower experimental force may be attributed to the actual lubrication condition, the actual flow stress of the annealed blank, and the elastic deformation of the press and die system. The trial results confirmed that the axially preloaded split die is feasible and that the numerical model captures the main process behavior.

I continued the production trial to evaluate die service life. After 50,000 extrusions, the die core showed no cracks, no fracture, and no severe wear. The split interface remained closed, and no drilling was observed. The common normal length of the forged gear blanks was measured at the first piece, at 25,000 pieces, and at 50,000 pieces. The results are listed in Table 15. The measured values remained within the design requirement of 32.30 mm with a tolerance of +0.06 mm. The progressive increase in the common normal length was small and stable. Based on the condition of the die after 50,000 pieces, the expected die life is more than 100,000 pieces. This service life is a significant improvement over the integral die and the transverse split die, both of which suffered from cracking or drilling.

Inspection stage Design requirement (mm) Measured common normal length (mm) Die condition
First piece 32.30 +0.06 32.30 to 32.32 Good
25,000 pieces 32.30 +0.06 32.31 to 32.33 Good
50,000 pieces 32.30 +0.06 32.32 to 32.34 No cracks or drilling

Discussion

The failure of cold extrusion dies for gears is governed by the interaction of high forming load, brittle core material, stress concentration at the tooth entrance, and the cyclic nature of production. My results show that increasing the radial interference alone cannot solve the problem because the axial tensile stress remains high. A transverse split can reduce the axial stress, but it introduces a new failure mode: blank metal drilling into the split gap. The axially preloaded split die solves this problem by applying the preload close to the split interface and by keeping the prestressing rings continuous. The continuous rings provide radial confinement, while the axial preload closes the split gap. The result is a die core that remains in compression and a split interface that remains sealed during extrusion.

The response surface optimization further improved the design. The optimized dimensions increased the die size only slightly, but they reduced the stress in the middle and outer rings and kept the core in compression. The optimized interference values were \(U_1=0.26\) mm and \(U_2=0.29\) mm. These values are practical for manufacturing and assembly. The selected entrance angle of 60 degrees and root width of 3.2 mm provided a good balance between tooth filling and die stress. The friction study confirmed that lubrication is critical for producing sound forged gear blanks and for protecting the die cavity.

From a mechanics point of view, the die design can be summarized by three requirements. First, the radial preload must be high enough to keep the core in compression under the internal forming pressure. Second, the axial clamping must be applied near the split interface to prevent gap opening. Third, the contact width must be small enough to generate a high contact pressure but large enough to avoid local crushing. These requirements can be expressed as

$$ \sigma_{\theta,\mathrm{core}} < 0, \qquad p_c = \frac{F}{k l_c} > p_{\mathrm{metal}}, \qquad \sigma_{\mathrm{contact}} = \frac{F}{k l_c} < \sigma_{\mathrm{allow}} $$

where \(p_{\mathrm{metal}}\) is the local pressure of the blank metal at the split interface and \(\sigma_{\mathrm{allow}}\) is the allowable contact stress of the die insert. The selected values \(F=65,000\) N, \(k=2.0\) mm, and \(p_c=2,237\) N/mm^2 satisfy these conditions for the present gear and press conditions. The die has been used in production, and the measured common normal length of the forged gear blanks remained within tolerance after 50,000 pieces.

Conclusions

I analyzed the failure modes of cold extrusion dies for a heavy-truck planetary spur gear and developed an axially preloaded split die design method. The main conclusions are as follows.

1. The integral three-layer die experiences a large tangential tensile stress of about 630 MPa and an axial tensile stress of about 278 MPa near the tooth entrance. These stresses exceed the safe limit of the cemented carbide core and cause cracking and fracture. Increasing the radial interference reduces the tangential stress but does not eliminate the axial tensile stress.

2. A transverse split die reduces the axial tensile stress, but the bolted preload generates a bending moment that opens the split interface. Blank metal enters the gap and produces a drilling defect. This defect makes the transverse split die unsuitable for producing forged gear blanks.

3. The axially preloaded split die applies the clamping force close to the split interface and keeps the prestressing rings continuous. With a contact width of 2.0 mm and an axial preload of 65,000 N, the contact pressure reaches about 2,237 N/mm^2. The split interface remains closed, no drilling occurs, and the core remains in compression.

4. Response surface optimization gave the best die dimensions: \(d_2=130\) mm, \(d_3=230\) mm, \(d_4=360\) mm, \(U_1=0.26\) mm, and \(U_2=0.29\) mm. The optimized die kept all ring stresses below the allowable values and improved material utilization.

5. The entrance half angle of 60 degrees, the entrance root width of 3.2 mm, and a low friction coefficient provided a good balance between tooth filling, forming load, and die stress. These parameters are recommended for industrial production of forged gear blanks with the axially preloaded split die.

6. The production trial produced forged gear blanks with complete tooth filling and no drilling. The measured forming force was 5,960 kN, about 9.1 percent lower than the simulated value. After 50,000 pieces, the die showed no cracks or fracture, and the common normal length remained within the design requirement. The expected die life exceeds 100,000 pieces. The experimental results confirm the feasibility of the axially preloaded split die and the validity of the numerical model.