I investigated a fractured screw gear that had been operating as the driven member of a worm transmission in a reducer. The screw gear failed after a short service interval, and several teeth were broken near the tooth root. Because the screw gear was made of a relatively soft tin bronze while the worm was made of a much harder alloy steel, the screw gear became the critical component in the transmission. I combined experimental failure analysis, three-dimensional solid modeling, dynamic contact finite element analysis, crack-tip stress intensity factor calculation, and strain-life fatigue analysis to explain the failure. The central question I addressed was whether the screw gear failed by high-cycle fatigue or by low-cycle fatigue, and how an initial crack at the screw gear root changed the fatigue life.

I began with the physical evidence because the fracture surface contained information about the loading history of the screw gear. The damaged region was not distributed uniformly around the screw gear. Instead, the failure was concentrated in one sector. In that sector, I observed twelve broken teeth, pronounced plastic deformation at the tooth ends, and severe damage in the middle tooth bodies. The first broken tooth appeared to be the leftmost tooth in the damaged zone. After that tooth fractured, the adjacent screw gear teeth were subjected to repeated impact from the worm, and the middle teeth underwent further plastic deformation before final fracture. The tooth at the right side of the damaged zone showed slight deformation but did not break, which suggested that the earlier broken teeth absorbed a significant part of the impact energy. This fracture pattern was consistent with an overloaded screw gear in which an initial crack or local damage had already formed before final rupture.
I performed chemical composition analysis to identify the screw gear material. The measured composition is summarized in Table 1. The tin content was high, and the alloy also contained zinc, iron, aluminum, nickel, manganese, and antimony. By comparing the measured values with the standard range for cast tin bronze, I identified the screw gear material as a 10-2 tin bronze, that is, ZCuSn10Zn2. This identification was important because the mechanical behavior of the screw gear, including its hardness, yield strength, and fatigue resistance, depended strongly on the bronze composition and microstructure.
| Element | Sn | Zn | Fe | Al | Ni | Mn | Sb |
|---|---|---|---|---|---|---|---|
| Screw gear | 10.098 | 1.252 | 0.043 | 0.005 | 0.360 | 0.012 | 0.048 |
| Standard | 2.0-11.0 | 1.0-3.0 | ≤0.5 | ≤0.02 | ≤2.5 | ≤0.2 | ≤0.3 |
I then prepared metallographic samples from the failed screw gear. The microstructure contained a white alpha solid solution matrix, gray-black tin-rich alpha solid solution along the dendrite boundaries, and gray script-like alpha plus delta eutectoid in the interdendritic regions. The alpha plus delta eutectoid was not uniformly distributed. It was coarse in some regions, fine in others, and generally less continuous than would be expected in a well-controlled casting. This microstructural inhomogeneity reduced the local hardness of the screw gear. When the alpha plus delta eutectoid is coarse and uneven, the screw gear cannot resist local plastic deformation as effectively, and the tooth root becomes more vulnerable to crack initiation under repeated contact loading.
The hardness measurements confirmed that the screw gear was softer than the worm. The Brinell hardness values are listed in Table 2. The average hardness of the failed screw gear was 75.5 HBW, which was below the minimum requirement of 80 HBW for ZCuSn10Zn2. The average hardness of the worm was 176.3 HBW, which satisfied the relevant requirement. The large hardness difference between the worm and the screw gear meant that the screw gear tooth surface yielded first when the contact stress exceeded the local strength. Under repeated meshing, this hardness mismatch promoted plastic deformation, surface damage, and crack initiation at the screw gear root.
| Component | Measurement 1 (HBW) | Measurement 2 (HBW) | Measurement 3 (HBW) | Average (HBW) |
|---|---|---|---|---|
| Screw gear failure zone | 75.1 | 75.9 | 75.5 | 75.5 |
| Worm | 175.9 | 177.2 | 175.8 | 176.3 |
Scanning electron microscopy gave direct evidence of cracking at the screw gear tooth root. I observed an initial crack with a size on the order of \(4 \times 10^{-4}\) m. The crack was located in a region that experienced repeated tensile and compressive loading during meshing. In a worm transmission, the screw gear tooth root does not experience a smooth constant load. Instead, it experiences alternating contact, bending, and sliding. When the initial meshing impact is large, the screw gear root can develop a small crack even before general surface fatigue appears. Once this crack exists, the repeated meshing load drives it forward. The crack reduces the effective load-bearing area of the screw gear tooth and eventually causes final fracture.
I established three-dimensional solid models of the worm and the screw gear to reproduce the transmission geometry. For the worm, I used the axial tooth profile of an Archimedes worm. The main geometric parameters are given in Table 3. The axial pitch, addendum, working depth, clearance, and root fillet were calculated from the module and standard relationships. The relevant formulas are shown below.
$$p_x = \pi m$$
$$h_a = m$$
$$h = 2m$$
$$c = 0.2m$$
$$p_f = 0.3m$$
| Parameter | Symbol | Unit | Value |
|---|---|---|---|
| Module | m | mm | 2.37 |
| Number of starts | z1 | — | 1 |
| Pressure angle | alpha | degree | 20 |
| Reference diameter | d1 | mm | 30.4 |
| Addendum | ha | mm | 2.37 |
| Working tooth height | h | mm | 4.74 |
| Axial pitch | px | mm | 7.442 |
| Clearance | c | mm | 0.474 |
| Root fillet radius | pf | mm | 0.711 |
For the screw gear, I used a bicubic B-spline surface representation of the tooth flank. The screw gear tooth surface is a conjugate surface generated by the worm hob. I described the motion of the hob tip points K1 and K2 in the screw gear coordinate system. The trajectory equations are given below.
$$x_2 = (A_0 – R_1 \cos\phi_1)\cos(\phi_2 \pm \Delta\phi_2)$$
$$y_2 = (A_0 – R_1 \cos\phi_1)\sin(\phi_2 \pm \Delta\phi_2)$$
$$z_2 = R_1 \sin\phi_1$$
$$\phi_2 = \frac{\phi_1}{i_{12}}$$
$$\Delta\phi_2 = \frac{|K_1K_2|}{2 p i_{12}}$$
$$\frac{|K_1K_2|}{2} = \frac{\pi m}{4} – \left( h_a^* m \tan\alpha_u + \frac{c}{1-\sin\alpha_u}\cos\alpha_u \right)$$
I used these equations to generate the screw gear tooth groove surface and then subtracted the groove from the screw gear blank. The resulting screw gear model had a curved tooth flank that matched the worm geometry. I assembled the worm and the screw gear with a center distance of 110 mm and a pressure angle of 20 degrees. The assembly was then transferred to the finite element environment for dynamic contact analysis.
In the finite element model, I simplified the transmission by retaining only the screw gear teeth and worm threads that participated in meshing. This reduced the mesh size without changing the local contact behavior. The material properties are listed in Table 4. I used a bilinear isotropic hardening model for both materials. The screw gear had a lower elastic modulus, lower yield strength, and lower hardness than the worm. Therefore, the screw gear was expected to accumulate plastic strain first.
| Property | Unit | ZCuSn10Zn2 screw gear | 20Cr steel worm |
|---|---|---|---|
| Elastic modulus | GPa | 103 | 200 |
| Density | kg/m3 | 8820 | 7850 |
| Poisson ratio | — | 0.34 | 0.30 |
| Yield strength | MPa | 284 | 550 |
| Tangent modulus | MPa | 1102 | 1450 |
I defined frictional contact between the worm thread surface and the screw gear tooth surfaces. The friction coefficient was 0.1. I used the augmented Lagrange method and set the geometric correction to add offset with no ramping. The worm was treated as the target body, and the screw gear teeth were treated as the contact bodies. For meshing, I used tetrahedral elements for the screw gear and hexahedral elements for the worm. The global element size was 2 mm, and the contact surfaces were refined to 0.5 mm. The final model contained 139286 elements and 211010 nodes.
I applied a rotational velocity to the worm and a resisting torque to the screw gear. The worm speed was 1470 rpm, and the screw gear torque was 572 N·m. I divided the simulation into three load steps. The first step established contact over a very short time of \(1 \times 10^{-5}\) s. The second step stabilized the contact transition over \(1 \times 10^{-4}\) s. The third step simulated the dynamic meshing process over 0.123 s, which covered the complete engagement of three screw gear teeth. This load-step strategy avoided rigid-body motion at the start of the analysis and allowed the contact stress to develop gradually.
The dynamic contact analysis showed that the maximum contact stress occurred on the left screw gear tooth during the initial meshing stage. The value was 308 MPa. Because the allowable contact stress of the screw gear material was 220 MPa, the computed stress was 40 percent higher than the allowable value. The middle screw gear tooth reached a maximum contact stress of 292 MPa, which was 5.5 percent lower than the left tooth. The right screw gear tooth reached 283 MPa, which was 8.8 percent lower than the left tooth. The stress results are summarized in Table 5. The left tooth was the most severely loaded, which agreed with the fracture observation that the leftmost tooth broke first.
| Screw gear tooth | Maximum contact stress (MPa) | Difference from left tooth (%) | Comparison with allowable stress |
|---|---|---|---|
| Left tooth | 308 | 0 | 40% above 220 MPa |
| Middle tooth | 292 | 5.5 lower | 32.7% above 220 MPa |
| Right tooth | 283 | 8.8 lower | 28.6% above 220 MPa |
I also extracted the contact stress history. In the single-tooth meshing region, the average contact stress was about 294 MPa, and the peak stress exceeded the allowable stress. In the double-tooth meshing region, the average contact stress dropped to about 97 MPa. Therefore, the screw gear experienced cyclic loading between a high-stress state and a low-stress state. This cyclic contact stress was the mechanical driving force for fatigue crack initiation at the screw gear root. The stress history had three peaks, corresponding to the three single-tooth meshing events in the simulation. The periodic fluctuation of the contact stress confirmed that the screw gear was not operating under a steady load.
I calculated the reaction force on the screw gear contact surface to obtain the load spectrum. The load spectrum is an essential input for fatigue life prediction. In the single-tooth meshing region, the average reaction force was 5872 N, the maximum was 6752 N, and the minimum was 4991 N. In the double-tooth meshing region, the average reaction force was 4085 N, the maximum was 4956 N, and the minimum was 3214 N. The load fluctuation was 15.99 percent in single-tooth meshing and 21.32 percent in double-tooth meshing. These values are listed in Table 6.
| Meshing region | Average force (N) | Maximum force (N) | Minimum force (N) | Fluctuation (%) |
|---|---|---|---|---|
| Single-tooth | 5872 | 6752 | 4991 | 15.99 |
| Double-tooth | 4085 | 4956 | 3214 | 21.32 |
The contact status analysis showed that the screw gear teeth were mainly in the sliding state during meshing. I did not observe extensive sticking. The contact line moved continuously across the screw gear tooth surface, and the contact area was largest in the single-tooth meshing region. The contact line length was approximately two-thirds of the screw gear face width in single-tooth meshing and decreased in double-tooth meshing. This behavior explained why the maximum stress and the maximum plastic deformation appeared near the tooth tip and why the fracture zone was localized.
I studied the influence of torque on the screw gear contact stress. I kept the worm speed constant and varied the screw gear torque. The results are given in Table 7. As the torque increased, the maximum contact stress increased significantly. When the torque was 572 N·m, the maximum contact stress was 308 MPa. When the torque was reduced to 171.6 N·m, the maximum contact stress fell to 190 MPa, which was below the allowable contact stress. The relationship between torque and contact stress could be approximated by a power-law form.
$$\sigma_H = a T^b$$
| Torque (N·m) | 572 | 514.8 | 457.6 | 400.4 | 343.2 | 286 | 228.8 | 171.6 |
|---|---|---|---|---|---|---|---|---|
| Maximum contact stress (MPa) | 308 | 302 | 295 | 265 | 241 | 222 | 208 | 190 |
I then studied the influence of worm speed. With the screw gear torque fixed, increasing the worm speed increased the contact stress. The results are listed in Table 8. At 1470 rpm, the maximum contact stress was 308 MPa. At 441 rpm, the maximum contact stress decreased to 201 MPa. The speed effect was slightly weaker than the torque effect, but it was still significant. The relationship could also be expressed as a power-law function.
$$\sigma_H = c n^d$$
| Worm speed (rpm) | 1470 | 1323 | 1176 | 1029 | 882 | 735 | 588 | 441 |
|---|---|---|---|---|---|---|---|---|
| Maximum contact stress (MPa) | 308 | 298 | 287 | 272 | 251 | 231 | 211 | 201 |
I also examined the influence of the screw gear tooth form. Two geometric parameters were varied: face width and module. The effect of face width is shown in Table 9. As the face width increased, the contact line length increased, and the maximum contact stress increased slightly. The effect was relatively mild. When the face width decreased from 20 mm to 6 mm, the maximum contact stress decreased from 308 MPa to 274 MPa.
| Face width (mm) | 20 | 18 | 16 | 14 | 12 | 10 | 8 | 6 |
|---|---|---|---|---|---|---|---|---|
| Maximum contact stress (MPa) | 308 | 303 | 299 | 293 | 289 | 284 | 278 | 274 |
The effect of module was much stronger. Table 10 shows that increasing the module reduced the maximum contact stress substantially. When the module increased from 2.37 mm to 3.77 mm, the maximum contact stress decreased from 308 MPa to 147 MPa. A larger module increased the tooth thickness and the local load-bearing capacity of the screw gear, which reduced stress concentration. For the same torque and speed, a larger-module screw gear was therefore much less likely to exceed the allowable contact stress.
| Module (mm) | 2.37 | 2.57 | 2.77 | 2.97 | 3.17 | 3.37 | 3.57 | 3.77 |
|---|---|---|---|---|---|---|---|---|
| Maximum contact stress (MPa) | 308 | 288 | 260 | 237 | 217 | 191 | 173 | 147 |
After the stress analysis, I inserted a semi-elliptical crack at the screw gear tooth root. The crack was described by a major radius and a minor radius. The major radius represented the crack width along the tooth width direction, and the minor radius represented the crack depth along the tooth height direction. I divided the crack front into fifteen segments, generated six contour rings around the front, and divided each ring into sixteen segments. This produced a refined crack-tip mesh. The crack model allowed me to calculate the stress intensity factors for Mode I, Mode II, and Mode III.
The stress intensity factors are fundamental quantities in linear elastic fracture mechanics. I used the following definitions.
$$K_I = \lim_{r\to 0} \sigma_{yy}\sqrt{2\pi r}$$
$$K_{II} = \lim_{r\to 0} \tau_{yx}\sqrt{2\pi r}$$
$$K_{III} = \lim_{r\to 0} \tau_{yz}\sqrt{2\pi r}$$
For a crack width of \(4 \times 10^{-4}\) m and a crack depth of \(3 \times 10^{-4}\) m, the Mode I stress intensity factor reached a maximum of 56.151 MPa·mm^0.5 at the crack front ends and a minimum of 40.92 MPa·mm^0.5 at the crack front center. The distribution was concave, with lower values in the middle and higher values at the two sides. The Mode II stress intensity factor reached a maximum of 32.597 MPa·mm^0.5 at the center and a minimum of -9.235 MPa·mm^0.5 at the ends. The Mode III stress intensity factor varied from -20.976 MPa·mm^0.5 at the left end to 18.311 MPa·mm^0.5 at the right end. These results are summarized in Table 11. Because the maximum Mode I value was much higher than the maximum Mode II and Mode III values, Mode I was the dominant crack propagation mode at the screw gear root.
| Mode | Maximum value | Location | Minimum value | Location | Distribution shape |
|---|---|---|---|---|---|
| Mode I | 56.151 MPa·mm^0.5 | Crack front ends | 40.92 MPa·mm^0.5 | Crack front center | Concave |
| Mode II | 32.597 MPa·mm^0.5 | Crack front center | -9.235 MPa·mm^0.5 | Crack front ends | Convex |
| Mode III | 18.311 MPa·mm^0.5 | Right end | -20.976 MPa·mm^0.5 | Left end | Linear increase |
I then varied the crack width while keeping the crack depth at 0.3 mm. The Mode I stress intensity factor increased as the crack width increased. The results are shown in Table 12. When the crack width increased from 0.15 mm to 0.4 mm, the center value increased from 22.146 MPa·mm^0.5 to 40.92 MPa·mm^0.5, while the end value increased from 51.348 MPa·mm^0.5 to 56.151 MPa·mm^0.5. The center increased much more rapidly than the ends. This showed that the crack growth rate along the width direction was higher than along the depth direction.
| Crack width (mm) | Center K_I (MPa·mm^0.5) | End K_I (MPa·mm^0.5) |
|---|---|---|
| 0.15 | 22.146 | 51.348 |
| 0.20 | 26.412 | 52.221 |
| 0.25 | 31.008 | 53.174 |
| 0.30 | 35.229 | 54.316 |
| 0.35 | 38.574 | 55.207 |
| 0.40 | 40.920 | 56.151 |
I also varied the crack depth while keeping the crack width at 0.4 mm. The results are listed in Table 13. For shallow cracks, the Mode I stress intensity factor distribution was convex, with a higher value at the center. For deeper cracks, the distribution became concave, with higher values at the ends. This transition showed that shallow cracks initially grew more readily in the depth direction, but once the crack became sufficiently deep, the width direction became the dominant growth direction. For the screw gear, the width-direction growth had a stronger influence on the remaining life.
| Crack depth (mm) | Center K_I (MPa·mm^0.5) | End K_I (MPa·mm^0.5) | Distribution shape |
|---|---|---|---|
| 0.05 | 48.831 | 8.484 | Convex |
| 0.10 | 51.226 | 21.335 | Convex |
| 0.15 | 54.094 | 38.318 | Convex |
| 0.20 | 40.920 | 48.712 | Concave |
| 0.25 | 43.571 | 52.016 | Concave |
| 0.30 | 45.962 | 56.151 | Concave |
For fatigue life prediction, I used nCode DesignLife. I imported the finite element stress results, the load spectrum, and the strain-life properties of the screw gear material. The software calculated the fatigue life by combining the local stress and strain history with the material fatigue curve. I used an E-N strain-life approach because the screw gear experienced local plastic deformation at the tooth root and because the presence of an initial crack shifted the failure mode toward low-cycle fatigue.
The strain-life relationship was described by the Coffin-Manson-Basquin equation. The total strain amplitude was the sum of the elastic strain amplitude and the plastic strain amplitude.
$$\frac{\Delta\varepsilon_t}{2} = \frac{\Delta\varepsilon_e}{2} + \frac{\Delta\varepsilon_p}{2} = \frac{\sigma_f’}{E}(2N_f)^b + \varepsilon_f'(2N_f)^c$$
$$\frac{\Delta\varepsilon_e}{2} = \frac{\sigma_f’}{E}(2N_f)^b$$
$$\frac{\Delta\varepsilon_p}{2} = \varepsilon_f'(2N_f)^c$$
The cyclic stress-strain behavior was described by the Ramberg-Osgood relationship.
$$\frac{\Delta\sigma}{2} = K’\left(\frac{\Delta\varepsilon_p}{2}\right)^{n’}$$
I obtained the fatigue parameters by fitting the simulated strain-life data. The parameters are listed in Table 14. The cyclic strain hardening exponent was 0.361, the cyclic strength coefficient was 571.980 MPa, the fatigue strength coefficient divided by the elastic modulus was 0.011, the fatigue strength exponent was -0.174, the fatigue ductility coefficient was 0.125, and the fatigue ductility exponent was -0.482.
| Parameter | Symbol | Value |
|---|---|---|
| Cyclic strain hardening exponent | n’ | 0.361 |
| Cyclic strength coefficient | K’ | 571.980 MPa |
| Fatigue strength coefficient divided by E | sigma_f’/E | 0.011 |
| Fatigue strength exponent | b | -0.174 |
| Fatigue ductility coefficient | epsilon_f’ | 0.125 |
| Fatigue ductility exponent | c | -0.482 |
I simulated the screw gear fatigue life for different torques and recorded the total strain amplitude, elastic strain amplitude, plastic strain amplitude, and the number of reversals to failure. The data are given in Table 15. As the strain amplitudes decreased, the fatigue life increased. The total strain amplitude decreased from 1.53 percent to 0.34 percent, and the number of reversals to failure increased from 162 to 11300. The plastic strain-life curve and the elastic strain-life curve intersected between 2172 and 5051 reversals.
| Reversals to failure 2N_f | Total strain amplitude (%) | Elastic strain amplitude (%) | Plastic strain amplitude (%) |
|---|---|---|---|
| 162 | 1.538 | 0.456 | 1.082 |
| 349 | 1.115 | 0.390 | 0.723 |
| 2172 | 0.571 | 0.290 | 0.321 |
| 5051 | 0.445 | 0.249 | 0.206 |
| 7210 | 0.395 | 0.234 | 0.165 |
| 11300 | 0.341 | 0.215 | 0.135 |
I derived the transition fatigue life by setting the elastic strain amplitude equal to the plastic strain amplitude. The transition life is the boundary between low-cycle fatigue and high-cycle fatigue for the screw gear material.
$$\frac{\Delta\varepsilon_e}{2} = \frac{\Delta\varepsilon_p}{2}$$
$$\frac{\sigma_f’}{E}(2N_f)^b = \varepsilon_f'(2N_f)^c$$
$$(2N_f)_t = \left( \frac{\varepsilon_f’}{\sigma_f’/E} \right)^{1/(b-c)}$$
$$(2N_f)_t = \left( \frac{0.125}{0.011} \right)^{1/(-0.174+0.482)} \approx 2673$$
The transition fatigue life was therefore 2673 reversals. This value was critical for interpreting the screw gear failure. The actual screw gear failed after approximately 55 cycles. Because 55 was far below 2673, the actual failure was a low-cycle fatigue failure. The finite element simulation without an initial crack predicted 3513 cycles, which was above 2673 and therefore classified as high-cycle fatigue. The difference between the simulation and the actual failure showed that the initial crack at the screw gear root was not a minor defect. It changed the failure mode from high-cycle fatigue to low-cycle fatigue.
I then predicted the fatigue life of the screw gear without a crack. The minimum life occurred on the left screw gear tooth and was 3513 cycles. The middle tooth had a life of 3794 cycles, and the right tooth had a life of 3892 cycles. The left tooth life was 7.4 percent lower than the middle tooth and 9.7 percent lower than the right tooth. This distribution agreed with the contact stress distribution and with the observed fracture order. However, 3513 cycles was still far below the engineering requirement of 10000 cycles.
I studied the effect of torque on fatigue life. The results are shown in Table 16. As the torque increased, the fatigue life decreased. When the torque was 572 N·m, the life was 3513 cycles. When the torque was reduced to 171.6 N·m, the life increased to 11054 cycles, which exceeded the engineering requirement. The torque effect was strong and approximately logarithmic.
| Torque (N·m) | 572 | 514.8 | 457.6 | 400.4 | 343.2 | 286 | 228.8 | 171.6 |
|---|---|---|---|---|---|---|---|---|
| Fatigue life (cycles) | 3513 | 4681 | 5714 | 6641 | 7715 | 8924 | 10157 | 11054 |
The effect of worm speed on fatigue life is shown in Table 17. Higher worm speed reduced the screw gear fatigue life. At 1470 rpm, the life was 3513 cycles. At 441 rpm, the life increased to 10876 cycles. The speed effect was comparable to the torque effect. For a screw gear operating under high speed and heavy load, reducing either the torque or the speed could significantly extend the life.
| Worm speed (rpm) | 1470 | 1323 | 1176 | 1029 | 882 | 735 | 588 | 441 |
|---|---|---|---|---|---|---|---|---|
| Fatigue life (cycles) | 3513 | 4913 | 6121 | 7215 | 8210 | 9143 | 10021 | 10876 |
I also evaluated the effect of screw gear face width on fatigue life. The results are given in Table 18. A smaller face width produced a longer fatigue life, but the improvement was moderate. When the face width decreased from 20 mm to 6 mm, the fatigue life increased from 3513 cycles to 6492 cycles. Even the smallest face width did not reach the engineering requirement of 10000 cycles. Therefore, face width alone was not sufficient to solve the screw gear fatigue problem.
| Face width (mm) | 20 | 18 | 16 | 14 | 12 | 10 | 8 | 6 |
|---|---|---|---|---|---|---|---|---|
| Fatigue life (cycles) | 3513 | 3962 | 4359 | 4701 | 5114 | 5513 | 6001 | 6492 |
The effect of module on fatigue life was much stronger. The results are shown in Table 19. When the module increased from 2.37 mm to 3.77 mm, the fatigue life increased from 3513 cycles to 15646 cycles. A module larger than 3.13 mm produced a life above 10000 cycles. This showed that increasing the module was an effective way to improve the load capacity and fatigue life of the screw gear. However, increasing the module also increased the size and mass of the screw gear, so the design had to balance life, size, and cost.
| Module (mm) | 2.37 | 2.57 | 2.77 | 2.97 | 3.17 | 3.37 | 3.57 | 3.77 |
|---|---|---|---|---|---|---|---|---|
| Fatigue life (cycles) | 3513 | 5301 | 7096 | 8501 | 10519 | 12251 | 13754 | 15646 |
I finally analyzed the effect of an initial crack on the screw gear fatigue life. The fatigue life was controlled by the crack at the tooth root rather than by the tooth tip contact. The results for different crack widths and depths are listed in Table 20. When the crack depth was held constant, increasing the crack width strongly reduced the fatigue life. When the crack width was held constant, increasing the crack depth also reduced the life, but the trend was gentler. This confirmed that crack growth in the width direction had a greater effect on the remaining life of the screw gear.
| Crack depth (mm) | Crack width 0.05 mm | Crack width 0.10 mm | Crack width 0.15 mm | Crack width 0.20 mm | Crack width 0.25 mm | Crack width 0.30 mm |
|---|---|---|---|---|---|---|
| 0.15 | 1214 | 1159 | 1101 | 1034 | 981 | 931 |
| 0.20 | 1001 | 952 | 901 | 847 | 781 | 719 |
| 0.25 | 874 | 811 | 749 | 672 | 617 | 563 |
| 0.30 | 661 | 606 | 542 | 471 | 427 | 371 |
| 0.35 | 479 | 412 | 354 | 299 | 255 | 212 |
| 0.40 | 281 | 229 | 172 | 125 | 87 | 49 |
When the crack width was \(4 \times 10^{-4}\) m and the crack depth was \(3 \times 10^{-4}\) m, the predicted fatigue life was 49 cycles. The actual screw gear failed after approximately 55 cycles, so the relative error was about 10.9 percent. This close agreement supported the conclusion that the initial crack at the screw gear root was the dominant cause of the low-cycle fatigue failure. Every crack size in the analyzed range produced a fatigue life below the transition life of 2673 cycles, which meant that the screw gear with a root crack was always in the low-cycle fatigue regime.
From the combined experimental and numerical results, I concluded that the screw gear failure was not caused by a single overload event alone. The soft bronze screw gear had a hardness below the standard requirement, and its microstructure contained uneven alpha plus delta eutectoid. The worm was much harder. Under the actual torque and speed, the contact stress on the screw gear exceeded the allowable value by about 40 percent. The initial meshing impact created a small crack at the screw gear root. The alternating contact and bending stress then drove the crack forward. Because the crack was present, the fatigue life dropped from the high-cycle range to the low-cycle range. The final fracture occurred after a short number of cycles, and the broken teeth showed plastic deformation and fatigue crack growth characteristics.
I also found that the fatigue life of the screw gear was most sensitive to torque, worm speed, module, and initial crack size. Reducing the torque from 572 N·m to 171.6 N·m increased the life by about 215 percent. Reducing the worm speed from 1470 rpm to 441 rpm increased the life by about 210 percent. Increasing the module from 2.37 mm to 3.77 mm increased the life by about 345 percent. Reducing the face width from 20 mm to 6 mm increased the life by about 85 percent. Among the geometric parameters, the module had a much stronger effect than the face width. Among the crack parameters, the crack width had a stronger effect than the crack depth. These trends provide practical guidance for the design and maintenance of screw gear transmissions.
For engineering practice, I would recommend several measures. First, the screw gear material should meet the hardness requirement, and the casting process should produce a uniform alpha plus delta eutectoid distribution. Second, the worm and screw gear should be matched so that the contact stress remains below the allowable value under the maximum torque. Third, if high torque and high speed are required, a larger module should be selected or the load should be reduced. Fourth, the screw gear root should be inspected for initial cracks, because even a very small crack can reduce the fatigue life from thousands of cycles to tens of cycles. Fifth, the load spectrum should be monitored in service, since the screw gear is subjected to cyclic single-tooth and double-tooth meshing loads rather than a constant load.
In summary, I used failure analysis, three-dimensional modeling, dynamic contact finite element analysis, crack-tip stress intensity factor calculation, and strain-life fatigue analysis to study a fractured screw gear in a worm transmission. The experimental results showed that the screw gear material was ZCuSn10Zn2 with low hardness and uneven microstructure. The finite element results showed that the screw gear root and tooth tip experienced contact stresses above the allowable value. The crack analysis showed that Mode I was the dominant crack mode and that crack growth along the width direction was faster than along the depth direction. The fatigue analysis showed that the transition life was 2673 cycles and that an initial crack of width \(4 \times 10^{-4}\) m and depth \(3 \times 10^{-4}\) m produced a life of 49 cycles, close to the observed 55 cycles. The failure was therefore a low-cycle fatigue failure of the screw gear, initiated by an initial root crack and driven by repeated meshing contact.