In our work on automotive drivetrain components, gear forging has become a central route for producing high-strength, lightweight, and durable rotating parts. The differential assembly is a clear example. A traditional differential uses several separate components: a drive spiral bevel gear, a driven spiral bevel gear, a coaxial drive cylindrical gear, a driven cylindrical gear, a differential housing, and a half-shaft connection system. Each part must carry torque, resist bending, and survive millions of load cycles. When we moved from a six-piece cast-and-forged assembly to an integrated combination gear forging, we changed both the product architecture and the manufacturing logic. The integrated gear forging replaces several bolted, welded, or shrink-fitted parts with one closed-die forged body. This shift reduces weight, lowers the number of joints, improves fatigue performance, and enables the differential housing function to be partly absorbed into the forged structure. In our development program, we used CAE simulation, die stress analysis, and trial production to optimize the gear forging process. The result is a robust gear forging route with stable material flow, longer die life, and reliable forming quality.

1. Product Function and Integrated Architecture

The differential receives torque from the transmission and distributes it to the wheels while allowing speed differences during turns. In the classic layout, the drive spiral bevel gear rotates the driven spiral bevel gear and completes the first reduction stage. The driven spiral bevel gear is coaxial with a drive cylindrical gear. Together they rotate and drive the driven cylindrical gear, which completes the second reduction stage. The driven cylindrical gear is mounted on the differential housing. When it rotates, the differential and half-shafts transmit motion to the wheels. The spiral bevel gear set therefore sits at the heart of the system. In our gear forging program, the main products include precision forgings for drive and driven spiral bevel gears, and these are produced with specialized, scaled, and lean methods.

The integrated combination gear forging combines several functions into one high-strength precision forged body. Instead of casting the differential housing and then assembling it with the driven spiral bevel gear, we forge the housing-related geometry and the gear-related geometry as a single connected structure. This integrated approach supports lightweight design because it removes redundant material, fasteners, and assembly interfaces. It also improves stiffness and load transfer. The closed-die gear forging process is used to form the complex shape, and CAE simulation is used to refine the product structure and process parameters. The optimized gear forging has better die life and more stable forming quality.

Function in the Differential Traditional Approach Integrated Gear Forging Approach Benefit
First reduction stage Separate spiral bevel gear pair Forged spiral bevel gear geometry integrated with adjacent features Higher torque density and fewer joints
Second reduction stage Separate cylindrical gear mounted on housing Combination gear forging with coaxial features Better alignment and stiffness
Differential housing Cast housing with machining Forged housing-related geometry combined with gear body Improved fatigue life and lightweight potential
Torque transmission Splines, bolts, welds, shrink fits Continuous forged material path Lower stress concentration and fewer failure sites
Manufacturing route Multiple cast and forged parts One integrated gear forging plus finishing Shorter assembly chain and lower logistics burden

2. Complexity and Design Challenge

The integrated gear forging is not a simple axisymmetric part. It has height steps, section changes, an internal bore, oil grooves, and stem features. The forging complexity coefficient is a useful first measure. We define it as:

$$S=\frac{M_f}{M_n}$$

where \(M_f\) is the mass or volume of the forging and \(M_n\) is the mass or volume of the circumscribed envelope. For this gear forging, the calculated value was \(S=0.28\), which places the part in the S3 category, meaning a relatively complex forging. A low complexity coefficient indicates that a large portion of the envelope is empty, so material must flow around corners, ribs, and recesses rather than simply filling a compact block. This is exactly why the gear forging required careful preform design and CAE simulation.

Parameter Symbol Value Interpretation
Forging mass \(M_f\) Reference value from solid model Actual metal required in the part
Envelope mass \(M_n\) Reference value from bounding volume Mass if the entire envelope were filled
Complexity coefficient \(S=M_f/M_n\) 0.28 S3 class, relatively complex
Main geometric risks Height drop, section change, oil grooves, stem steps High Local die wear and folding risk
Critical non-machined surfaces Oil grooves and pocket recesses High Defects cannot be removed by machining

The initial gear forging design had a closed-die forging route. Because the shape was complex, the height difference and cross-section change were large, and local die wear was severe. The three oil grooves in the internal bore and the two pocket recesses at the stem steps were forged surfaces. Among these, the oil grooves suffered the most serious wear and were prone to fatigue cracks. The oil grooves also created a large height drop and a complex local shape, so material was very likely to fold during extrusion. Folding is especially dangerous in gear forging because it creates a lap or crack-like defect that can act as a stress raiser under cyclic torque.

3. Initial Gear Forging Process Route

Our first process route was straightforward but required precise control at every step:

Blanking → heating → preforming → closed-die forging → punching → inspection.

The equipment set included a circular saw for blanking, an induction furnace for heating, a hydraulic press for preforming, a 2500 t friction press for closed-die gear forging, and a punch press for punching. This route was selected because it matches the medium-to-large batch production of automotive gear forgings and provides good dimensional repeatability when the tooling is properly maintained.

Step Operation Equipment Key Control Purpose
1 Blanking Circular saw Diameter, length, mass tolerance Provide accurate forging volume
2 Heating Induction furnace Temperature, time, atmosphere Lower flow stress and improve forgeability
3 Preforming Hydraulic press Thickness, diameter, symmetry Distribute material before closed-die forging
4 Closed-die forging 2500 t friction press Blow energy, die temperature, lubrication Fill the gear forging cavity and form non-machined features
5 Punching Punch press Coaxiality, burr, hole quality Remove the web or bore slug
6 Inspection Gauges, optical instruments, NDT Dimensions, defects, microstructure Confirm gear forging quality

The blank was selected after precise calculation, solid modeling, and finite element analysis. A round bar with a diameter of about 120 mm was suitable for production. The blank mass was controlled within a tolerance of about ±0.1 kg. Small-batch trials confirmed that this blank specification met the production requirements and it was released to the process sheet. For gear forging, the blank mass is not a minor detail. If the blank is too small, the cavity will not fill and the forging will be scrapped. If the blank is too large, flash increases, die load rises, and material utilization falls.

The basic mass balance for the gear forging can be written as:

$$V_b = V_f + V_{flash} + V_{scale} + V_{loss}$$

where \(V_b\) is the blank volume, \(V_f\) is the finished forging volume, \(V_{flash}\) is the flash volume, \(V_{scale}\) is the scale loss, and \(V_{loss}\) is other loss such as trimming and punching. The material utilization is:

$$\eta_m = \frac{m_f}{m_b}\times 100\% = \frac{V_f}{V_b}\times 100\%$$

For an integrated gear forging, a high \(\eta_m\) is desirable, but it must not come at the cost of incomplete filling or internal defects. The optimal balance is found by simulation and trial forging.

4. Material and Thermal Parameters

The forging material for the simulation study was a carburizing alloy steel grade represented by 8620. In production, a similar medium-carbon alloy steel such as 20CrMnTi can also be used when the hardenability and case depth requirements match the final gear application. The hot working window is important because the material must flow into the oil grooves and stem features without developing surface defects.

Parameter Value or Range Unit Effect on Gear Forging
Material type 8620 or equivalent carburizing steel — Good core toughness and case hardenability
Forging temperature range 1050–1200 °C Lower flow stress, better cavity filling
Final forging temperature 950 °C Prevent grain growth and cold die loading
Heating method Induction furnace — Fast, controlled, repeatable heating
Heating rate 43 pieces per hour pcs/h Matches press cycle and reduces temperature loss
Die temperature 150–300 °C Reduce thermal shock and improve metal flow
Lubrication Graphite spray — Lower friction and assist release
Temperature check Optical pyrometer — Detect overheating or low-temperature blanks

The heating operation used an induction furnace with a controlled cycle. We checked temperature with an optical pyrometer and recorded the results. A three-way sorting system removed bars that did not meet the temperature requirement. This is essential for gear forging because overheating can cause burning, coarse grains, and hot tears, while underheating raises flow stress and may cause incomplete fill, die overload, or cracking.

5. Closed-Die Gear Forging Mechanics

Closed-die gear forging forces metal to fill a cavity that defines the gear teeth, oil grooves, steps, and bore-related features. The material flow is not free; it is constrained by the die walls. The local flow stress controls the pressure required to fill the cavity. A common constitutive expression for hot deformation is:

$$\bar\sigma = K \bar\varepsilon^n \dot{\bar\varepsilon}^m \exp\left(\frac{Q}{RT}\right)$$

where \(\bar\sigma\) is the effective flow stress, \(\bar\varepsilon\) is the effective strain, \(\dot{\bar\varepsilon}\) is the effective strain rate, \(T\) is the absolute temperature, \(Q\) is the activation energy, \(R\) is the gas constant, and \(K\), \(n\), and \(m\) are material constants. In hot gear forging, the exponential temperature term is very influential. A small drop in temperature can significantly increase the required forging load.

The effective strain is often calculated as:

$$\bar\varepsilon = \sqrt{\frac{2}{3}\varepsilon_{ij}\varepsilon_{ij}}$$

and the effective strain rate as:

$$\dot{\bar\varepsilon} = \sqrt{\frac{2}{3}\dot\varepsilon_{ij}\dot\varepsilon_{ij}}$$

The forging force can be estimated by:

$$F = K_f \sigma_y A_p$$

where \(K_f\) is a constraint factor, \(\sigma_y\) is the flow stress, and \(A_p\) is the projected area. For a complex gear forging, \(K_f\) increases with friction, aspect ratio, and local constraint. A more detailed expression for a simple upsetting case is:

$$K_f = 1 + \frac{0.4\mu D}{H}$$

where \(\mu\) is the friction coefficient, \(D\) is the diameter, and \(H\) is the height. In the integrated gear forging, the oil grooves and stem steps act as local constraints that raise the pressure required for filling. This is why the oil groove geometry had such a strong effect on die wear and defect formation.

Mechanical Variable Symbol Role in Gear Forging Practical Control
Effective strain \(\bar\varepsilon\) Measures accumulated deformation Limit excessive local strain to avoid folding
Effective strain rate \(\dot{\bar\varepsilon}\) Controls flow stress and temperature rise Match press speed and blow energy
Flow stress \(\bar\sigma\) Determines forging load and die pressure Maintain proper temperature
Friction coefficient \(\mu\) Affects material flow and die wear Use graphite lubrication and clean dies
Projected area \(A_p\) Scales forging force Control flash and preform shape
Die contact pressure \(p\) Drives wear and fatigue cracking Optimize radii, taper, and preform

6. CAE Simulation of Gear Forging

To verify the optimized design, we used CAE software to simulate the forging process. The simulation used the same process parameters for both the initial and optimized structures, except for the upper die geometry. This allowed a direct comparison of material flow, defect formation, die stress, and filling behavior. The main simulation parameters are listed below.

Simulation Parameter Value Unit Comment
Blank material 8620 — Carburizing alloy steel
Heating temperature 1150 °C Within hot forging window
Die temperature 300 °C Preheated tooling
Upper die speed 100 mm/s Representative press speed
Number of blows 1 — Single-blow forming to avoid repeated loading defects
Friction coefficient 0.3 — Hot forging with graphite lubrication
Mesh type Updated Lagrangian tetrahedral or hexahedral mesh — Automatic remeshing for large deformation
Contact condition Rigid dies, deformable workpiece — Die stress evaluated separately

The simulation tracked the velocity field, strain field, temperature field, and contact pressure. A useful damage indicator for ductile fracture and folding tendency is the normalized Cockcroft–Latham integral:

$$\int_0^{\bar\varepsilon_f} \frac{\sigma_1}{\bar\sigma} d\bar\varepsilon = C$$

where \(\sigma_1\) is the maximum principal stress, \(\bar\sigma\) is the effective stress, \(\bar\varepsilon_f\) is the effective strain at fracture, and \(C\) is a critical value. A high local value of this integral indicates a high risk of cracking or folding. In the initial design, the oil groove region showed a strong tendency for flow line convergence and surface lap formation.

We also evaluated the temperature evolution using a simple lumped thermal model:

$$T(t) = T_\infty + (T_0 – T_\infty)e^{-ht}$$

where \(T_0\) is the initial temperature, \(T_\infty\) is the environment or die temperature, and \(h\) is a cooling coefficient. In actual forging, the surface cools quickly on contact with the die, while the interior remains hotter. This thermal gradient changes flow stress and can cause the surface layer to fold if the local geometry forces it to reverse direction.

7. Defect Formation in the Initial Design

The initial gear forging had three oil grooves in the bore and two pocket recesses at the stem step. During closed-die forging, the upper die had three protrusions that first contacted the preform. These protrusions formed the bottom of the oil groove region. As the upper die continued downward, the bottom of the preform was compressed and material began to flow upward toward the large outer diameter. At the same time, some material flowed toward the oil groove location. The two flow fronts met, creating turbulence and a folded surface.

This defect is a classic folding problem in gear forging. The material does not simply fill the cavity; it creates a lap where the surface folds back on itself. The lap may be partly welded under high pressure and temperature, but it remains a discontinuity. After heat treatment and service loading, it can become a fatigue initiation site. Because the oil grooves are non-machined surfaces, the defect cannot be removed by later cutting. This makes the forging process itself responsible for the final surface integrity.

Defect Feature Initial Design Behavior Root Cause Risk
Oil groove lap Visible folding above the groove Opposing material flow fronts meet and fold Fatigue crack initiation
Die wear at oil grooves Local severe wear and fatigue marks High contact pressure and sharp geometry Short die life and dimensional drift
Stem step flow Step creates回流-like reversal Sharp section change and dead metal zone Incomplete fill or internal lap
Local die stress High stress concentration Small radii and steep taper Die cracking and repair downtime

We modified the product structure after reviewing the simulation results. The goal was to reduce the opposing flow, guide the metal in one preferred direction, and eliminate sharp transitions. The optimized design was discussed with the customer and approved for trial. In the optimized gear forging, the oil groove location still contacts the die first, but the triangular structure allows metal to flow simultaneously toward the gear teeth and the lower stem. The oil groove region no longer creates a direct flow collision, so the forging forms well without folding defects.

8. Geometry Optimization for Gear Forging

The optimization followed three main principles: reduce resistance, eliminate reverse flow, and smooth stress raisers. These principles are general for any complex gear forging, but they were applied here to the specific oil groove and stem geometry.

Optimization Measure Initial Geometry Optimized Geometry Expected Effect
Oil groove top Small arc and steep taper Larger arc and gentler taper Lower flow resistance and better metal mobility
Bottom step Step-like transition Triangular transition Eliminate reverse flow during extrusion
Connection radii Sharp or small radii Larger, blended radii Reduce die stress and improve die life
Flow path Opposing flow fronts Continuous flow to gear and stem Prevent folding and lap formation
Die contact pressure High local peaks More uniform distribution Lower wear rate and longer die life
Forging defect risk High Low Stable production and better fatigue life

The optimized oil groove top uses a larger radius and a controlled taper. This reduces the local constraint and allows the metal to move more freely into the groove. The bottom step was changed from a stepped structure to a triangular structure. The triangular shape acts like a flow guide. It avoids the dead zone that caused the material to reverse direction. Finally, the connection points between the oil groove, stem, and main body were blended with larger arcs. This reduces the stress concentration factor, which can be approximated by:

$$K_t = 1 + 2\sqrt{\frac{t}{r}}$$

where \(t\) is a characteristic section thickness and \(r\) is the fillet radius. Increasing \(r\) reduces \(K_t\), which lowers the peak die stress and improves fatigue resistance of the tooling. The same logic applies to the forged part: smoother transitions reduce stress concentration in service.

After the geometry change, we ran the CAE simulation again. The optimized gear forging filled completely. There was no underfill, no missing material, and no folding. The oil groove region formed cleanly. The stem region also filled without a lap. The simulation showed that the optimized design had a more balanced velocity field and a more uniform effective strain distribution. The maximum contact pressure on the die was reduced, especially at the oil groove corners.

9. Die Stress, Wear, and Life Improvement

Die life is a major cost driver in gear forging. The oil grooves and stem steps are local features that concentrate stress and wear. We evaluated die life using contact pressure, sliding distance, and temperature. A simplified Archard wear model is:

$$V_w = K_w \frac{F_n L}{H}$$

where \(V_w\) is the wear volume, \(K_w\) is the wear coefficient, \(F_n\) is the normal load, \(L\) is the sliding distance, and \(H\) is the hardness of the die material. The wear depth can be estimated by dividing the wear volume by the worn area:

$$h_w = \frac{V_w}{A_w}$$

For the initial design, the oil groove corners had high \(F_n\) and long local sliding distance because the material had to reverse and fold. After optimization, the triangular transition and larger radii reduced \(F_n\) and shortened the sliding distance in the critical zone. The die temperature also became more uniform because the material flow was smoother and the contact pressure was distributed over a larger area.

Die Life Factor Initial Design Optimized Design Improvement Mechanism
Peak contact pressure High at oil groove corners Lower and more uniform Larger radii and triangular flow guide
Local sliding distance Long due to flow reversal Shorter and more direct Continuous flow path
Thermal load Local hot spots More balanced temperature Better contact distribution
Fatigue crack risk High Reduced Lower stress concentration
Die maintenance interval Short Extended Less wear and fewer repairs
Dimensional stability Poor over time Better over time Slower wear rate

The optimized gear forging die life improved significantly. This is not only a tooling benefit. Longer die life means fewer interruptions, more consistent dimensions, and lower scrap. In high-volume gear forging, even a small improvement in die life can produce a large cost reduction. It also improves the repeatability of the oil groove geometry, which is a non-machined surface and therefore directly affects the final part performance.

10. Forging Process Parameter Window

After optimization, we defined a process window for production. The window covers heating, preforming, forging, punching, and lubrication. The goal is to keep material flow stable and avoid both underfill and folding. For a complex gear forging, the process window is not a single point; it is a range with controls at each step.

Stage Parameter Target Upper Limit Lower Limit Reason
Blanking Mass Nominal ±0.1 kg +0.1 kg −0.1 kg Control volume and flash
Heating Temperature 1150 °C 1200 °C 1050 °C Avoid burning and cold forging
Heating Cycle 43 pcs/h Variation < 5% Variation < 5% Match press rhythm
Preforming Die preheat 150–300 °C 300 °C 150 °C Reduce thermal shock
Preforming Thickness By stroke control Upper tolerance Lower tolerance Ensure proper preform volume distribution
Closed-die forging Blow count 1 1 1 Avoid multiple-blow defects
Closed-die forging Die temperature 150–300 °C 300 °C 150 °C Improve flow and die life
Closed-die forging Lubrication Graphite spray each cycle Uniform No dry spots Control friction and release
Punching Coaxiality Within drawing Max deviation Min deviation Ensure bore quality

The single-blow condition is important. The simulation showed that one blow is sufficient to fill the optimized cavity. Multiple blows can cause repeated loading, local cooling, and additional shear, which may increase the risk of folding or cracking. We also clean the die cavity with an air jet after each forging and apply graphite lubricant. This removes scale, debris, and excess lubricant that could otherwise be pressed into the oil groove surface.

11. Production Equipment and Tooling

The production line for the integrated gear forging uses standard forging equipment arranged for stable flow. The 2500 t friction press is the central machine. It provides the required energy for a single-blow closed-die forging. The hydraulic press for preforming controls the preform shape, which is critical for directing metal into the gear teeth and oil grooves. The induction furnace provides fast heating with low scale. The punch press completes the bore.

Equipment Function Key Specification Role in Gear Forging
Circular saw Blanking Accurate length and mass Provides the correct forging volume
Induction furnace Heating 43 pcs/h, controlled temperature Delivers hot, uniform blanks
Hydraulic press Preforming Stroke-controlled thickness Distributes material before closed-die forging
2500 t friction press Closed-die forging Single blow, high energy Forms complex gear and oil groove geometry
Punch press Punching Precise coaxiality Creates the bore and removes slug
Die set Tooling Preheated, lubricated, cleaned Defines the gear forging shape
Optical pyrometer Temperature check Non-contact measurement Prevents overheat or underheat
Three-way sorter Temperature sorting Accept, rework, reject Removes nonconforming blanks

Tooling design is equally important. The die inserts must be preheated to 150–300 °C before production. The preheating reduces thermal shock and helps the first forgings fill correctly. The die cavity must be cleaned after every cycle. Any scale or graphite buildup in the oil groove region can change the local geometry and increase the risk of a lap. The punch tooling must maintain coaxiality to avoid an off-center bore and uneven wall thickness.

12. Quality Control and Inspection

Quality control for the integrated gear forging covers dimensions, surface defects, microstructure, hardness, and internal soundness. Because the oil grooves are forged surfaces, visual inspection and surface defect detection are especially important. We also check the bore, stem, and gear tooth region for fill and cracks.

Quality Characteristic Method Frequency Acceptance Criterion Action if Nonconforming
Overall dimensions Gauges and calipers Each batch and periodic sampling Within drawing tolerance Adjust die or process
Oil groove surface Visual and magnifying inspection High frequency No lap, fold, crack, or underfill Stop and inspect die and preform
Bore coaxiality Punch fixture and gauge Periodic Within coaxiality tolerance Check punch alignment
Hardness Hardness tester After heat treatment Within specified range Review heat treatment cycle
Microstructure Metallographic section Process qualification and audit Fine grain, no excessive decarburization Adjust heating and forging temperature
Internal defects Ultrasonic or magnetic particle testing as required Sampling or 100% for critical parts No unacceptable indications Segregate and analyze
Mass and volume Scale or weighing Startup and periodic Within blank tolerance Adjust blanking

We treat the oil groove as a critical feature. A defect there can survive machining because the groove is not machined. This makes the forging operation directly responsible for the fatigue performance of the final gear. The inspection plan therefore includes a dedicated check for the oil groove surface after forging. If a lap or fold is found, we stop production and inspect the die, the preform, and the heating temperature. In most cases, a lap indicates that the preform volume distribution or die surface condition has changed.

13. Trial Production Validation

After the CAE simulation showed that the optimized design formed well, we conducted trial production. The trial used the same process route and equipment as the planned production line. The initial design and optimized design were both forged for comparison. The initial design showed a clear folding defect above the oil groove where the material contacted the flat surface. The optimized design showed no such defect.

Trial Item Initial Design Optimized Design Result
Cavity fill Complete but with local lap Complete and sound Optimized design passes
Oil groove surface Visible folding above groove Clean surface, no fold Major quality improvement
Stem step flow Flow reversal tendency Triangular flow guide works No lap or dead zone
Die wear appearance Local severe wear More uniform wear Longer die life
Forging load High local pressure Reduced peak pressure More stable press operation
Dimensional repeatability Variable due to wear Improved Better batch consistency
Post-forging inspection Defects found No unacceptable defects Customer approval

The trial results matched the simulation. This gave us confidence that CAE simulation is a reliable tool for gear forging development. It allowed us to test the initial design, identify the folding mechanism, change the geometry, and verify the improvement before cutting new dies. The trial also confirmed that the single-blow process with the optimized geometry is stable. The forged oil groove surface was clean, and the stem step filled without a lap.

14. Economic and Lightweight Benefits

The integrated gear forging supports lightweight design because it replaces a multi-part cast-and-forged assembly with a single high-strength forged structure. The weight reduction comes from several sources: fewer fasteners, less assembly material, better section efficiency, and the ability to place material only where it is needed. The forged material also has a continuous grain flow that follows the load path, which improves fatigue strength compared with a cast structure.

The material utilization can be expressed as:

$$\eta_m = \frac{m_f}{m_b}\times 100\%$$

The energy required for forging can be approximated by:

$$E = \int F \, ds$$

where \(F\) is the forging force and \(s\) is the ram displacement. A well-designed preform reduces unnecessary flash and lowers the required energy. The optimized gear forging reduces the peak force and distributes the deformation more evenly, which lowers the energy per part and reduces die wear.

Economic Factor Traditional Multi-Part Route Integrated Gear Forging Route Benefit
Part count Six separate components One integrated forging plus finishing Fewer joints and assembly steps
Weight Higher due to fasteners and cast sections Lower with forged optimized sections Lightweight vehicle design
Material utilization Lower due to separate blanks Higher with controlled preform and flash Less scrap and lower material cost
Die life Not applicable or lower for separate tools Improved by geometry optimization Lower tooling cost per part
Fatigue performance Joint-limited Continuous forged grain flow Longer service life
Production stability Assembly variation Single forging process with CAE control Better dimensional consistency
Development cycle Multiple prototypes and assembly trials CAE-guided gear forging trials Shorter and less wasteful

From a manufacturing perspective, the optimized gear forging reduces the risk of scrap caused by folding. Scrap is expensive not only because of lost material but also because of lost press time, heating energy, and labor. By eliminating the lap defect, we improved yield and reduced the need for rework or rejection. The longer die life also reduces downtime and tool maintenance cost. These factors combine to make the integrated gear forging economically attractive for high-volume automotive production.

15. Lessons for Future Gear Forging Programs

This project produced several lessons that we now apply to other gear forging developments. First, complexity should be evaluated early. The complexity coefficient \(S=M_f/M_n\) is simple but useful. A low value warns that material flow will be difficult and that preform design deserves extra attention. Second, CAE simulation should be used before die manufacturing. In this case, the simulation revealed the folding mechanism in the oil groove region and allowed us to change the geometry before trial. Third, sharp steps and small radii are not acceptable in complex gear forging. They create dead zones, reverse flow, high contact pressure, and short die life. Fourth, non-machined surfaces must be treated as critical surfaces. The oil grooves are forged surfaces, so any defect there remains in the final part. Fifth, process control must be tight. Temperature, blank mass, preform thickness, die temperature, lubrication, and die cleaning all influence the final gear forging quality.

We also learned that the die geometry and product geometry cannot be optimized separately. The oil groove top radius, taper, and triangular transition were product changes, but they directly affected die stress and material flow. In gear forging, product design and process design are coupled. A change that improves the part may also improve the tooling, and a change that helps the tooling may improve the part. The best result comes from evaluating both together with CAE and trial validation.

Lesson Technical Basis Recommended Action
Evaluate complexity early Low \(S\) means difficult filling Use preform design and simulation from the start
Simulate before cutting dies Folding and die stress can be predicted Run CAE for initial and optimized designs
Avoid sharp steps Steps cause reverse flow and dead zones Use triangular or tapered transitions
Increase radii and taper Reduces flow resistance and stress concentration Apply generous fillets at oil grooves and connections
Control non-machined surfaces Defects cannot be removed later Inspect oil grooves at high frequency
Maintain process discipline Temperature and lubrication affect flow Use optical pyrometry, sorting, and graphite spraying
Link product and process design Geometry affects die life and flow Optimize together with CAE and trials

16. Conclusion

Our integrated combination gear forging replaces a traditional multi-part differential assembly with a single high-strength precision forged structure. The gear forging route uses closed-die forging, CAE simulation, controlled heating, preforming, single-blow forging, and punching. The initial design had a complexity coefficient of 0.28 and was classified as relatively complex. The oil grooves and stem steps created severe local die wear and a high risk of folding. CAE simulation showed that opposing material flow fronts met in the oil groove region and formed a lap. We optimized the oil groove top with a larger arc and gentler taper, replaced the bottom step with a triangular transition, and increased the connection radii. The optimized gear forging filled completely without folding. Die stress and wear were reduced, and die life improved. Trial production confirmed the simulation results. The optimized gear forging has better quality, longer tool life, lower scrap, and improved lightweight potential. In future gear forging programs, we will continue to use complexity evaluation, CAE simulation, geometry optimization, and disciplined process control to produce robust integrated forgings for differential and drivetrain applications.